254 SMO / F44 – UNS S31254

6Mo super-austenitic stainless steel with nitrogen

Download data sheet (PDF)

Super-austenitic stainless with 6% Mo and 0.2% N, with pitting and crevice resistance in seawater comparable to that of costlier nickel alloys. Mechanical strength superior to 316L thanks to nitrogen.

Technical review Oct 2026 · minimum values per the cited standard; physical properties are typical; values marked * to be confirmed in the standard

FamilySuper austenitic stainless
UNSS31254
W.Nr. / EN1.4547 (X1CrNiMoCuN20-18-7)
PREN≈ 42 – 45 (typical ≈ 43)

Designations and equivalents

Designations of 254 SMO / F44 – UNS S31254
SystemDesignation
UNS S31254
W.Nr./EN 1.4547 (X1CrNiMoCuN20-18-7)
DIN X1CrNiMoCuN20-18-7
JIS SUS312L
Trade names 254 SMO (Outokumpu), 6Mo
Others SS 2378

Standards by product form

Standards for 254 SMO / F44 – UNS S31254
FormStandard
Bar ASTM A276 / A479
Forging/flange ASTM A182 F44
Plate ASTM A240
Tube ASTM A312 / A269 / A249
Fittings ASTM A403 WPS31254

Tolerances and HS codes

  • Forged bars (round and square): machining allowance from 2 mm (Ø 6–16 mm) to 24 mm (Ø 400–500 mm) on the diameter. E.g. Ø 100–125 mm finished: +7 mm, tolerance +6 / −0 (length up to 3,500 mm).
  • Forged discs: allowance of 4 to 9 mm on the diameter and 3 to 11 mm on the height, plus-only tolerance.
  • Cutting and machining: band saw −0 / +5 to +15 mm on length; waterjet +10 % of thickness on the diameter (min. 2 mm); machined parts −0 / +2 to +5 mm on the diameter. See the full tables (INF 002 and INF 003, the same for every alloy).
Tariff classification of 254 SMO / F44: NCM, HS, HTS and CN by product form
FormNCM (Brazil, 8 digits)HS (international, 6 digits)HTS (USA, 10 digits)*CN (European Union, 8 digits)*
Forged bar7222.30.007222.307222.30.00247222 30 51
Hot-rolled bar7222.11.007222.117222.11.00597222 11 11
Plate (> 10 mm, width ≥ 600 mm)7219.21.007219.217219.21.00207219 21 10
Seamless pipe7304.41.907304.417304.41.60457304 41 00
Welded pipe7306.40.007306.407306.40.50857306 40 80
Flange and fitting7307.21.007307.217307.21.50007307 21 00

Tariff class: stainless steel (by chemical composition, under the Chapter 72 Notes and Section XV Note 5).

*: US and EU codes for reference. NCM per current legislation (General Rules of Interpretation, Notes to Chapters 72, 74 and 75 and Section XV Note 5). Confirm the final code with your customs broker according to the item size and finish. HS = first 6 digits of the NCM.

Chemical composition (%)

ASTM A182 F44 / A240

Chemical composition of 254 SMO / F44 – UNS S31254, per ASTM A182 F44 / A240
ElementRange (%)
C ≤ 0.020
Mn ≤ 1.00
P ≤ 0.030
S ≤ 0.010
Si ≤ 0.80
Cr 19.5 – 20.5
Ni 17.5 – 18.5
Mo 6.0 – 6.5
Cu 0.50 – 1.00
N 0.18 – 0.25
Fe balance

Calculate the PREN of 254 SMO / F44 in the PREN calculator →

Mechanical properties

Solution annealed (ASTM A182 F44)

Mechanical properties of 254 SMO / F44 – UNS S31254
PropertyValue
Yield strength (0.2%) ≥ 300 MPa
Tensile strength ≥ 650 MPa
Elongation ≥ 35%
Reduction of area ≥ 50%
Hardness ≤ 223 HBW (A240)

Typical physical properties

Typical values at 20 °C
PropertyValue
Density 8.0 g/cm³
Melting range ≈ 1,320 – 1,390 °C
Modulus of elasticity 195 GPa
Thermal conductivity (20 °C) 14 W/m·K
Thermal expansion (20–100 °C) 16.5 µm/m·K

Calculate the weight of 254 SMO / F44 bar, plate or pipe →

Heat treatment, welding and machining

ItemUsual practice
Service temperature Cryogenic up to ≈ 400 °C (risk of intermetallic phases above).
Heat treatment Solution annealing 1,150 – 1,200 °C with rapid water quench.
Welding Good, with a Mo over-alloyed consumable: AWS ERNiCrMo-3 or ERNiCrMo-13 (electrodes ENiCrMo-3/-12); avoid matching-composition consumables because of Mo segregation.
Machining Machinability lower than carbon steel: it work hardens quickly; use sharp tools, positive rake, constant feed without 'rubbing' and abundant coolant. More difficult to machine than 316L because of the N and Mo.

Plan an open-die forging in 254 SMO / F44: reduction, slenderness and how much material to send →Simulate the cutting plan of the ingot or bar →

Filler metal for welding

The wire composition is usually not identical to the material: each page explains why.

Typical applications

  • Seawater systems (piping, pumps, exchangers)
  • Offshore: injection water and firefighting
  • Pulp and paper bleaching
  • Desalination
  • Gas scrubbers (FGD)
  • Chemical industry with halides

Alternatives: 904L in less aggressive media; super duplex (F55) with higher mechanical strength; Alloy 625 or C-276 above the pitting/crevice limit of 6Mo.

Compare alloys by corrosive medium, concentration and temperature →

254 SMO / F44: complete guide

What 254 SMO steel is

254 SMO belongs to the family of special stainless steels, in the "6Mo" group. It is an iron-chromium-nickel-molybdenum alloy with nitrogen, not a copper-nickel alloy: copper enters at only 0.5 – 1.0%. The designation F44 is that of the ASTM A182 forging standard, and 254 SMO is Outokumpu's trade name.

Chemical composition and role of the elements

Molybdenum (6.0 – 6.5%) and nitrogen (0.18 – 0.25%) are the elements that make the difference: the PREN, calculated as Cr + 3.3 Mo + 16 N, is between 42 and 45, versus 23 – 28 for 316L. Nitrogen also raises the yield strength to twice that of 316L and stabilizes the austenite. The high nickel (17.5 – 18.5%) is needed to keep the austenitic structure with so much chromium and molybdenum.

Heat treatment and welding

Supplied solution annealed at 1,150 – 1,200 °C and water quenched, a higher temperature than for common austenitics in order to dissolve the sigma and chi phases that molybdenum promotes. Welding is done without preheating and without post-weld heat treatment, but necessarily with a nickel-alloy consumable such as ERNiCrMo-3 (625), because a weld with a matching consumable segregates molybdenum and loses pitting resistance. Dustre performs solution annealing in its own furnaces as part of its heat treatment service.

Corrosion and limits of use

It resists natural and chlorinated seawater, brines, acidic solutions with chlorides and bromides, and gas desulfurization media. It is an alloy for aqueous corrosion: the ASME code allows it up to about 400 °C, and prolonged exposure above 600 °C precipitates intermetallic phases that embrittle the material.

Applications

Seawater heat exchangers and piping, desalination plants, FGD absorbers, pulp bleaching equipment, offshore components and pump and valve parts for severe chlorides. Alternatives: 904L for less severe media and super duplex F53 when more mechanical strength is needed.

Supply forms and Dustre services

Round bars and blocks forged in open die, cut to size on a band saw, with rough or finish machining, solution annealing in our own furnaces and hardness, tensile and impact testing. All material is supplied with a 3.1 inspection certificate and heat traceability.

Frequently asked questions

What is the chemical composition of 254 SMO / F44?

Per ASTM A182 F44 / A240: C ≤ 0.020; Mn ≤ 1.00; P ≤ 0.030; S ≤ 0.010; Si ≤ 0.80; Cr 19.5 – 20.5.

Which standards cover 254 SMO / F44?

Bar: ASTM A276 / A479. Forging/flange: ASTM A182 F44. Plate: ASTM A240. Tube: ASTM A312 / A269 / A249. Fittings: ASTM A403 WPS31254.

Up to what temperature can 254 SMO / F44 be used?

Cryogenic up to ≈ 400 °C (risk of intermetallic phases above).

Which materials can replace 254 SMO / F44?

904L in less aggressive media; super duplex (F55) with higher mechanical strength; Alloy 625 or C-276 above the pitting/crevice limit of 6Mo.

Where to buy 254 SMO / F44 in Brazil?

Dustre supplies 254 SMO / F44 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

Need 254 SMO / F44?Bars, forgings and parts with EN 10204 3.1 certificate.

Forms and stock of 254 SMO / F44

Dustre supplies 254 SMO / F44 as bar, plate, pipe and tube, forgings and flanges and fittings, cut to size, with forged and machined parts to drawing (shafts, discs, rings and blocks) and a 3.1 certificate.

Not in stock at the moment: supplied to order, with lead time in the quotation.

See the full ready-to-ship stock · Request a quote for 254 SMO / F44

Where to buy 254 SMO / F44 in Brazil?

Dustre supplies 254 SMO / F44 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

See also

HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp

We use your data only to answer this quote. Privacy. · WhatsApp +55 11 98649-0075 · Mon–Thu 07:00–17:00 · Fri 07:00–16:00 (Brasília time)