Super duplex 2507 / F53 stainless steel
UNS S32750, 1.4410
Super duplex 2507 is austenitic-ferritic stainless UNS S32750 (about 50/50 ferrite and austenite), with 24–26 % Cr, 3–5 % Mo and 0.24–0.32 % N, designed for PREN ≥ 40 and a yield strength of 550 MPa, twice that of austenitics. In forgings and flanges it is ASTM A182 F53; in EN, 1.4410; as a casting, grade 5A (CE3MN). F55 (S32760, Zeron 100) is another super duplex, with copper and tungsten, and has its own page.
One composition, several standards
The name changes with the product form. When specifying, cite the standard, grade and class.
| Form | ASTM/ASME | Grade/class | EN | ABNT/others |
|---|---|---|---|---|
| Forging and flange (B16.5) | A182 / SA-182 | F53 (S32750) | EN 10250-4 / EN 10222-5: 1.4410* | NORSOK M-630 MDS D54 |
| Bar | A479 / SA-479; A276 | S32750 | EN 10088-3 / EN 10272: 1.4410 | NORSOK MDS D57; JIS G4303 SUS327L1 (S32750)* |
| Plate, coil, strip | A240 / SA-240 | S32750 | EN 10088-2 / EN 10028-7: 1.4410 | NORSOK MDS D55; JIS G4304 SUS327L1* |
| Seamless pipe (line) | A790 / SA-790 | S32750 | EN 10216-5: 1.4410 | NORSOK MDS D51 |
| Heat exchanger tube | A789 / SA-789 | S32750 | EN 10216-5 | NORSOK MDS D58 |
| Welded pipe | A790 (welded); A928 (fusion welded, classes 1–5) | S32750 | EN 10217-7: 1.4410 | NORSOK MDS D52 |
| Fittings (butt-weld) | A815 / SA-815 | WPS32750 (classes WP-S, WP-W, WP-WX, CR)* | EN 10253-4 | NORSOK MDS D53 |
| Casting | A890 / A995 (pressure) | 5A = CE3MN (J93404) | EN 10213 / EN 10283: 1.4469 GX2CrNiMoN26-7-4 | NORSOK MDS D56 |
| Welding consumable | AWS A5.9 / A5.4 / A5.22 | ER2594, E2594, E2594T | EN ISO 14343: 25 9 4 N L | ASME IX: P-No. 10H |
| Washer/bolt, sour service | A182 / A479 / A276 + NACE | S32750 | — | NACE MR0175/ISO 15156-3; NACE MR0103; API 6A* |
NBR 5601 has no super duplex grade; specify by UNS + ASTM/EN product standard.
Tolerances and HS codes
- Forged bars (round and square): machining allowance from 2 mm (Ø 6–16 mm) to 24 mm (Ø 400–500 mm) on the diameter. E.g. Ø 100–125 mm finished: +7 mm, tolerance +6 / −0 (length up to 3,500 mm).
- Forged discs: allowance of 4 to 9 mm on the diameter and 3 to 11 mm on the height, plus-only tolerance.
- Cutting and machining: band saw −0 / +5 to +15 mm on length; waterjet +10 % of thickness on the diameter (min. 2 mm); machined parts −0 / +2 to +5 mm on the diameter. See the full tables (INF 002 and INF 003, the same for every alloy).
| Form | NCM (Brazil, 8 digits) | HS (international, 6 digits) | HTS (USA, 10 digits)* | CN (European Union, 8 digits)* |
|---|---|---|---|---|
| Forged bar | 7222.30.00 | 7222.30 | 7222.30.0024 | 7222 30 51 |
| Hot-rolled bar | 7222.11.00 | 7222.11 | 7222.11.0059 | 7222 11 11 |
| Plate (> 10 mm, width ≥ 600 mm) | 7219.21.00 | 7219.21 | 7219.21.0020 | 7219 21 10 |
| Seamless pipe | 7304.41.90 | 7304.41 | 7304.41.6045 | 7304 41 00 |
| Welded pipe | 7306.40.00 | 7306.40 | 7306.40.5085 | 7306 40 80 |
| Flange and fitting | 7307.21.00 | 7307.21 | 7307.21.5000 | 7307 21 00 |
Tariff class: stainless steel (by chemical composition, under the Chapter 72 Notes and Section XV Note 5).
*: US and EU codes for reference. NCM per current legislation (General Rules of Interpretation, Notes to Chapters 72, 74 and 75 and Section XV Note 5). Confirm the final code with your customs broker according to the item size and finish. HS = first 6 digits of the NCM.
Chemical composition by standard (%)
The ranges of each standard side by side, to see where they differ.
| Standard / grade | C max | Mn max | P max | S max | Si max | Cr | Ni | Mo | N | Others |
|---|---|---|---|---|---|---|---|---|---|---|
| A240/A182 F53 (S32750) | 0.030 | 1.20 | 0.035 | 0.020 | 0.80 | 24.0–26.0 | 6.0–8.0 | 3.0–5.0 | 0.24–0.32 | Cu 0.50 max |
| A890/A995 5A (CE3MN) | 0.03 | 1.50 | 0.04 | 0.04 | 1.00 | 24.0–26.0 | 6.0–8.0 | 4.0–5.0 | 0.10–0.30 | — |
| EN 1.4410 (X2CrNiMoN25-7-4) | 0.030 | 2.00 | 0.035 | 0.015 | 1.00 | 24.0–26.0 | 6.0–8.0 | 3.0–4.5 | 0.24–0.35 | — |
Calculate the PREN of Super duplex 2507 / F53 / S32750 in the PREN calculator →
Mechanical properties by standard
Minimum values at room temperature, in the stated delivery condition.
| Standard and condition | YS min | UTS | Elong. | RA | Hardness |
|---|---|---|---|---|---|
| FORGINGS | |||||
| A182 F53, solution annealed, ≤ 50 mm | 550 MPa (80 ksi) | 800 MPa min (116 ksi) | 15 % | not specified | 310 HBW max |
| A182 F53, > 50 mm | 515 MPa (75 ksi) | 730 MPa min (106 ksi) | 15 % | — | 310 HBW max |
| ROLLED | |||||
| A240 S32750, plate | 550 MPa | 795 MPa min | 15 % | — | 310 HBW / 32 HRC max |
| PIPE, FITTINGS AND CASTINGS | |||||
| A790 / A789 S32750 | 550 MPa | 800 MPa min | 15 % | — | 300 HBW / 32 HRC max |
| A890 / A995 5A (CE3MN) | 515 MPa (75 ksi) | 690 MPa min (100 ksi) | 18 % | — | — |
| FITTINGS | |||||
| A815 WPS32750 | per starting material* | 800 MPa min | 15 % | — | * |
Calculate the weight of Super duplex 2507 / F53 / S32750 bar, plate or pipe →
F53 (S32750) vs. F55 (S32760): 2507 vs. Zeron 100
Both alloys share the same 25Cr-7Ni base and the same 550 MPa YS. S32750 (2507) uses more Mo (up to 5 %) and N (0.24–0.32 %) and has no W; it has a higher minimum UTS (800 MPa) and lower elongation (15 %). S32760 (Zeron 100) adds Cu and W (0.5–1.0 % each), has Mo max 4 % and carries PREN ≥ 40 as a requirement in the composition itself; UTS sits at 750–895 MPa with 25 % elongation. In practice they are interchangeable in many MDS (NORSOK lists both on the same data sheet), but they are not the same grade: check which UNS the specification requires, and use a compatible consumable (ER2594 or Zeron 100X type).
Heat treatments required by the standards
| Standard | Delivery condition | Temperature |
|---|---|---|
| A182 F53 / A240 S32750 | Solution annealed and rapidly cooled in water or liquid medium | 1025 °C min (1880 °F); A240: 1025–1125 °C* |
| A890 / A995 5A | Solution annealed and water quenched | 1120 °C min* |
Plan an open-die forging in Super duplex 2507 / F53 / S32750: reduction, slenderness and how much material to send →Simulate the cutting plan of the ingot or bar →
Variants in the family
| Variant | Standards | Difference | YS / UTS |
|---|---|---|---|
| S32750 (2507, SAF 2507, 1.4410) | A182 F53, A240, A479, A790, A789, A815, A928 | Mo 3–5 %, N 0.24–0.32 %, no W/Cu | 550 / 800 MPa |
| S32760 (Zeron 100, 1.4501) | A182 F55, A240, A276, A479, A790, A789, A815, A928 | Cu 0.5–1 % and W 0.5–1 %; PREN ≥ 40 required | 550 / 750–895 MPa |
| S32550 (Ferralium 255, 1.4507) | A182 F61, A240, A479, A276, A790 | Cu 1.5–2.5 %, lower Ni and N; minimum PREN may be < 40 | 550 / 750–760 MPa |
| S32520 (UR 52N+, Ferralium 255-SD50, 1.4507) | A182 F59, A240, A789, A790, A928 | Cu 0.5–3 %*, N up to 0.35 %; PREN > 40 | 550 / 770 MPa |
| CE3MN (5A, J93404) | A890 / A995 5A | Casting equivalent to 2507; Mo 4–5 % | 515 / 690 MPa |
| CD3MWCuN (6A, J93380) | A890 / A995 6A | Casting equivalent to Zeron 100 (Cu + W) | 450 / 690 MPa |
Corrosion, PREN and temperature
- PREN: Cr + 3.3 Mo + 16 N. At the ASTM minimums S32750 may give ~38; that is why offshore purchases require PREN ≥ 40 calculated on the heat.
- Pitting and crevice corrosion: the usual test is ASTM G48 method A at 50 °C for 24 h, no pitting (22Cr: 40 °C). Typical CPT well above that of 22Cr duplex and 316L.
- Intermetallic phases (sigma, chi): precipitate quickly between ~600 and 1000 °C; the critical formation range goes from ~320 to 955 °C (A923). Slow cooling after solution annealing or welding with high heat input collapses toughness and pitting resistance.
- 475 °C embrittlement: the ferrite hardens with long exposure between ~300 and 525 °C, which limits continuous use to about 250 °C (ASME usually accepts up to ~315 °C)*.
- Low temperature: toughness proven by Charpy at −46 °C (NORSOK: 45 J average / 35 J individual) or −40 °C (A923 method B).
- NACE MR0175/ISO 15156-3: solution-annealed super duplex is accepted with pH2S, chloride and temperature limits that depend on the PREN range (40–45); NACE MR0103 limits super duplex to 32 HRC; NORSOK purchases usually require 28 HRC / 270 HB*.
Compare alloys by corrosive medium, concentration and temperature →
Tests required for super duplex (ASTM A923, G48, NORSOK)
- ASTM A923: detects intermetallic phases: method A (NaOH etch, acceptance only), method B (Charpy) and method C (ferric chloride).
- A923 method C: S32750, S32550 and S32520 tested at 40 °C, maximum loss 10 mdd.
- A923 method B: S32750 at −40 °C with energy agreed between purchaser and supplier; casting J93404 (5A) at −46 °C, 54 J min.
- ASTM G48 A at 50 °C / 24 h: no pitting and mass loss ≤ 4 g/m² is the usual NORSOK M-630/M-650 criterion*.
- Ferrite (ASTM E562): 35–55 % in base metal; in the weld, 30–70 % (NORSOK M-601)*.
- NORSOK M-650: manufacturer qualification (forge, foundry, mill) for 25Cr; requires a qualification piece with the tests above.
Welding
| Item | Usual practice |
|---|---|
| Consumable | ER2594 (AWS A5.9), E2594 (A5.4), E2594T (A5.22); EN ISO 14343 25 9 4 N L |
| Gas | Ar + 2 % N2 (shielding) and Ar or Ar + N2 for purging, to avoid nitrogen loss at the root |
| Preheat | Not used |
| Interpass | Max 100–150 °C (100 °C common for 25Cr)* |
| Heat input | Low and controlled, ~0.5–1.5 kJ/mm, to balance ferrite without precipitating sigma* |
| PWHT | No stress relief is done; if needed, only full solution annealing with water quenching |
| Control | Ferrite and hardness in qualification (350 HV10 max usual), G48 and Charpy per NORSOK M-601/M-650* |
Filler metal for welding
The wire composition is usually not identical to the material: each page explains why.
International equivalents
| System | Designation |
|---|---|
| UNS | S32750; equivalent casting J93404 (5A) |
| ASTM forging | F53 (S32750) |
| EN / W.Nr. | 1.4410 X2CrNiMoN25-7-4; cast 1.4469 GX2CrNiMoN26-7-4 |
| Trade names | SAF 2507 (Alleima), Forta SDX 2507 (Outokumpu), UR 2507 |
| JIS | SUS327L1 (≈ S32750) |
| GB | 022Cr25Ni7Mo4N / S25073 (≈ S32750) |
| ABNT / SAE / AISI | No AISI/SAE designation; NBR 5601 has no corresponding grade* |
Equivalence is by approximate composition; minimum properties, tests and heat treatment change from standard to standard.
Typical applications
| Form or industry | Where it is used |
|---|---|
| Offshore oil and gas | Seawater lines, injection, manifolds, umbilicals and firewater systems (NORSOK) |
| Subsea | Connectors, F53 flanges, hubs and valves in contact with seawater |
| Desalination (SWRO) | High-pressure pipes and vessels with brine |
| Chemicals and pulp | Exchangers, pumps and equipment with chlorides and acids |
| Pumps and valves | Cast 5A bodies, shafts and internals in A479 bar |
| Fastening | Super duplex studs and nuts for chloride and H2S service |
Frequently asked questions
Are F53 and F55 the same thing?
No. F53 is S32750 (2507) and F55 is S32760 (Zeron 100, with Cu and W). They have the same 550 MPa YS and 25Cr base, but composition, UTS and heat treatment differ.
What is the minimum PREN of 2507?
Market practice and NORSOK require PREN ≥ 40. At the ASTM minimums S32750 may give about 38, so the PREN must be calculated on the heat and stated on the certificate.
What is the difference between duplex and super duplex?
22Cr duplex (S31803/S32205, F51/F60) has PREN ~34 and YS 450 MPa. 25Cr super duplex has PREN ≥ 40 and YS 550 MPa, for seawater and more aggressive chlorides.
Which casting corresponds to 2507?
ASTM A890/A995 grade 5A (CE3MN, J93404).