Heat treatments of steels and alloys: which to use and what for

Each heat treatment combines temperature, time and cooling method to reach a property: more hardness, more toughness, more machinability or more corrosion resistance.

Technical review Oct 2026 · Sources: ASTM A182, A370, A564, A480, ASME VIII Div. 1 (UCS-56), ASM Handbook vol. 4

Comparison of the treatments

Heat treatments: typical temperature, cooling and purpose
TreatmentTypical temperature*CoolingPurposeAlloys
AnnealingAbove the critical range (carbon steel ~800–900 °C)Slow, in the furnaceSoften and ease machiningCarbon and alloy steels
Normalizing~850–950 °CIn airRefine and homogenize the grainA105, A350 LF2, alloy steels
QuenchingAustenitizing (4140 ~840–870 °C)Water, oil or polymerHarden (martensite)4140, 4340, F22, stainless 410/420/431
Tempering~150–700 °C, depending on hardnessIn airTrade hardness for toughnessEvery quenched steel
Solution annealingAustenitic stainless ~1040–1120 °C; duplex ~1020–1100 °CFast, in waterDissolve carbides and sigma phase, restore corrosion resistance304L, 316L, 904L, duplex, super duplex, 625, C-276
Aging17-4PH 480–620 °C (H900 to H1150)In airPrecipitation hardening17-4PH, 15-5PH, 718, K-500
Stress reliefCarbon steel ≥ 595 °C (post-weld)Slow, controlledReduce welding and machining stressesFabrications, welded parts

* Typical ranges. Temperature, time and medium come from the material standard or the customer specification.

Precautions by family

  • Duplex (including super duplex): never leave the part too long between ~600 and 1000 °C; it forms sigma phase and loses toughness and corrosion resistance. Cool quickly after solution annealing.
  • Austenitic stainless: between ~450 and 850 °C sensitization occurs; hence solution annealing and the use of "L" grades.
  • Cr-Mo steels (F11, F22, F91): F91 requires normalizing and tempering with strict temperature control.
  • Confirm the result: hardness, tensile and Charpy in the laboratory.

Frequently asked questions

What is the difference between tempering and annealing?

Tempering comes after quenching and reduces part of the hardness to gain toughness. Annealing is done on non-quenched material to soften it and ease machining or forming.

Why solution anneal duplex and stainless after forging?

Forging and slow cooling form carbides and intermetallic phases that reduce corrosion resistance and toughness. Solution annealing dissolves these phases and the fast cooling prevents them from returning.

Heat treatment with reportOwn furnaces, right after forging and machining.
Request a quote
HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp

We use your data only to answer this quote. Privacy. · WhatsApp +55 11 98649-0075 · Mon–Thu 07:00–17:00 · Fri 07:00–16:00 (Brasília time)