316 / 316L stainless steel: standards, composition and properties

316, 316L, 316H, 316Ti, 316LN and 316LVM · UNS S31600, S31603, S31609, S31635, S31653 · F316L, CF8M, CF3M, 1.4404

Download data sheet (PDF)

316 is the Cr-Ni austenitic stainless steel with 2 to 3 % molybdenum, which gives it resistance to chlorides and reducing acids far superior to 304. The same composition gets different names depending on the product form: TP316L for pipe, F316L for forgings, WP316L for fittings, CF3M when cast and 1.4404 in the European standard. The L, H, Ti, N/LN and LVM variants change carbon, nitrogen, titanium or cleanliness to suit welding, high temperature, strength or surgical implants.

Technical review Oct 2026 · * value to be confirmed in the current edition of the standard

UNSS31600 (316), S31603 (316L), S31609 (316H), S31635 (316Ti), S31651 (316N), S31653 (316LN), S31673 (316LVM)
CastCF8M (J92900) and CF3M (J92800), ASTM A351 / A743 / A744
EN / W.Nr.1.4401, 1.4404, 1.4571, 1.4435, 1.4436, 1.4429; cast 1.4408 / 1.4409; implant 1.4441
Base chemistry16–18 Cr, 10–14 Ni, 2–3 Mo, C ≤ 0.08 (L ≤ 0.030)
Typical PREN≈ 25 (316/316L); ≈ 26 (1.4435 / 316LVM)

One composition, several standards

The name changes with the product form. When specifying, cite the standard, grade and class.

Standards for 316 / 316L stainless by product form
FormASTM/ASMEGrade/classENABNT/others
Plate, coil, strip A240 / SA-240316, 316L, 316H, 316Ti, 316N, 316LNEN 10088-2; EN 10028-7 (pressure): 1.4401, 1.4404, 1.4571, 1.4435, 1.4429NBR 5601 (316, 316L, 316Ti*); AMS 5524 (316), AMS 5507 (316L); JIS G4304/G4305 SUS316/316L
Bar and section A276 (general), A479 / SA-479 (pressure vessels)316, 316L, 316H, 316Ti, 316N, 316LNEN 10088-3; EN 10272 (pressure)AMS 5648 (316), AMS 5653 (316L); JIS G4303 SUS316/316L
Forging and flange A182 / SA-182; A336 (heavy forgings); A965 (high temperature)F316, F316L, F316H, F316Ti, F316N, F316LNEN 10222-5: 1.4401, 1.4404, 1.4571, 1.4429ASME B16.5 flanges: group 2.2 (316, 316H, CF8M, CF3M) and 2.3 (316L)
Seamless and welded pipe A312 / SA-312; A358 (welded, large diameter); A376 (high temperature)TP316, TP316L, TP316H, TP316Ti, TP316N, TP316LNEN 10216-5 (seamless), EN 10217-7 (welded)AMS 5573 (seamless 316 tubing); JIS G3459 SUS316TP
Heat exchanger and boiler tube A213 / SA-213 (seamless), A249 / SA-249 (welded), A269 (general), A270 (sanitary)TP316, TP316L, TP316H, TP316TiEN 10216-5, EN 10217-7JIS G3463 SUS316TB
Welding fittings A403 / SA-403 (butt-weld), A182 (forged socket/threaded)WP316, WP316L, WP316H, WP316LNEN 10253-4MSS SP-43 (light)
Casting A351 / SA-351 (pressure), A743 (general), A744 (corrosion)CF8M (≈316), CF3M (≈316L), CF3MN (≈316LN)EN 10213: 1.4408 (GX5CrNiMo19-11-2), 1.4409 (GX2CrNiMo19-11-2)JIS G5121 SCS14A / SCS16A
Surgical implant ASTM F138 (bar, wire), F139 (sheet, strip)316LVM (UNS S31673)ISO 5832-1; 1.4441 (X2CrNiMo18-15-3)ABNT NBR ISO 5832-1
Welding consumable AWS A5.9 (wire), A5.4 (covered electrode)ER316L, ER316LSi, ER316H, E316L-16, ER318*EN ISO 14343: 19 12 3 L (Si)—

EN 1.4401/1.4404 require Mo 2.00–2.50 % (ASTM accepts 2.00–3.00 %); to guarantee Mo ≥ 2.5 % under the European standard, specify 1.4435 or 1.4436.

Tolerances and HS codes

  • Forged bars (round and square): machining allowance from 2 mm (Ø 6–16 mm) to 24 mm (Ø 400–500 mm) on the diameter. E.g. Ø 100–125 mm finished: +7 mm, tolerance +6 / −0 (length up to 3,500 mm).
  • Forged discs: allowance of 4 to 9 mm on the diameter and 3 to 11 mm on the height, plus-only tolerance.
  • Cutting and machining: band saw −0 / +5 to +15 mm on length; waterjet +10 % of thickness on the diameter (min. 2 mm); machined parts −0 / +2 to +5 mm on the diameter. See the full tables (INF 002 and INF 003, the same for every alloy).
Tariff classification of 316 / 316L stainless: NCM, HS, HTS and CN by product form
FormNCM (Brazil, 8 digits)HS (international, 6 digits)HTS (USA, 10 digits)*CN (European Union, 8 digits)*
Forged bar7222.30.007222.307222.30.00247222 30 51
Hot-rolled bar7222.11.007222.117222.11.00597222 11 11
Plate (> 10 mm, width ≥ 600 mm)7219.21.007219.217219.21.00207219 21 10
Seamless pipe7304.41.907304.417304.41.60457304 41 00
Welded pipe7306.40.007306.407306.40.50857306 40 80
Flange and fitting7307.21.007307.217307.21.50007307 21 00

Tariff class: stainless steel (by chemical composition, under the Chapter 72 Notes and Section XV Note 5).

*: US and EU codes for reference. NCM per current legislation (General Rules of Interpretation, Notes to Chapters 72, 74 and 75 and Section XV Note 5). Confirm the final code with your customs broker according to the item size and finish. HS = first 6 digits of the NCM.

Chemical composition by standard (%)

The ranges of each standard side by side, to see where they differ.

Chemical composition of 316 / 316L stainless by standard, in %
Standard / gradeCMnP maxS maxSi maxCrNiMoNOthers
ASTM A240 316 (S31600) 0.08 max2.00 max0.0450.0300.7516.0–18.010.0–14.02.00–3.000.10 max—
ASTM A240 316L (S31603) 0.030 max2.00 max0.0450.0300.7516.0–18.010.0–14.02.00–3.000.10 max—
ASTM A240 316H (S31609) 0.04–0.102.00 max0.0450.0300.7516.0–18.010.0–14.02.00–3.00—ASTM grain size No. 7 or coarser
ASTM A240 316Ti (S31635) 0.08 max2.00 max0.0450.0300.7516.0–18.010.0–14.02.00–3.000.10 maxTi 5×(C+N) min, 0.70 max
ASTM A240 316LN (S31653) 0.030 max2.00 max0.0450.0300.7516.0–18.010.0–14.02.00–3.000.10–0.16316N (S31651): same N with C 0.08 max
EN 10088-2 1.4404 (X2CrNiMo17-12-2) 0.030 max2.00 max0.0450.0151.0016.5–18.510.0–13.02.00–2.500.10 max1.4401: C 0.07 max; 1.4571: C 0.08, Ni 10.5–13.5, Ti 5×C to 0.70
EN 10088-2 1.4435 (X2CrNiMo18-14-3) 0.030 max2.00 max0.0450.0151.0017.0–19.012.5–15.02.50–3.000.10 max1.4429 (316LN): N 0.12–0.22, Ni 11.0–14.0
ASTM A351 CF8M (J92900) 0.08 max1.50 max0.0400.0401.5018.0–21.09.0–12.02.00–3.00—CF3M (J92800): C 0.03 max, Cr 17.0–21.0, Ni 9.0–13.0
ASTM F138 316LVM (S31673) 0.030 max2.00 max0.0250.0100.7517.00–19.0013.00–15.002.25–3.000.10 maxCu 0.50 max; Cr + 3.3 Mo ≥ 26.0

Calculate the PREN of 316 / 316L stainless in the PREN calculator →

Mechanical properties by standard

Minimum values at room temperature, in the stated delivery condition.

Minimum mechanical properties of 316 / 316L stainless
Standard and conditionYS minUTSElong.RAHardness
FORGINGS
A182 F316 / F316H / F316Ti, solution annealed 205 MPa (30 ksi)515 MPa min (75 ksi)30 %50 % (F316Ti: 40 %)not specified
A182 F316L, solution annealed 170 MPa (25 ksi)485 MPa min (70 ksi)30 %50 %not specified
A182 F316LN, solution annealed 205 MPa (30 ksi)515 MPa min (75 ksi)30 %50 %not specified
A182 F316N, solution annealed 240 MPa (35 ksi)550 MPa min (80 ksi)30 %50 %not specified
ROLLED (PLATE AND BAR)
A240 316 / 316H / 316Ti / 316LN, solution annealed 205 MPa (30 ksi)515 MPa min (75 ksi)40 %—217 HBW / 95 HRB max
A240 316L, solution annealed 170 MPa (25 ksi)485 MPa min (70 ksi)40 %—217 HBW / 95 HRB max
A240 316N, solution annealed 240 MPa (35 ksi)550 MPa min (80 ksi)35 %—217 HBW / 95 HRB max
A276 / A479 316, annealed 205 MPa (30 ksi)515 MPa min (75 ksi)30 % (A479); 40 % (A276 hot rolled)*40 % (A479); 50 % (A276)*—
EN 10088-2 1.4404, plate (P ≤ 75 mm) 220 MPa520–670 MPa45 %——
EN 10088-3 1.4404 / 1.4401, bar ≤ 160 mm 200 MPa500–700 MPa40 %——
ASTM F138 316LVM, annealed 190 MPa490 MPa min40 %——
ASTM F138 316LVM, cold worked 690 MPa*860 MPa min*12 %*——
PIPE, FITTINGS AND CASTINGS
A312 TP316 / TP316H, solution annealed 205 MPa (30 ksi)515 MPa min (75 ksi)35 % long. / 25 % transv.——
A312 TP316L, solution annealed 170 MPa (25 ksi)485 MPa min (70 ksi)35 % long. / 25 % transv.——
A213 TP316 / TP316H / TP316Ti 205 MPa (30 ksi)515 MPa min (75 ksi)35 %—192 HBW / 90 HRB max
A213 TP316L 170 MPa (25 ksi)485 MPa min (70 ksi)35 %—192 HBW / 90 HRB max
A403 WP316 / WP316L 205 / 170 MPa515 / 485 MPa min28 % long.——
A351 CF8M and CF3M, solution annealed 205 MPa (30 ksi)485 MPa min (70 ksi)30 %—not specified

Calculate the weight of 316 / 316L stainless bar, plate or pipe →

316 vs. 316L vs. 316H vs. 316Ti: what changes is the carbon

316 has C up to 0.08 %; when welded or heated between ~425 and 815 °C it precipitates chromium carbides at the grain boundaries (sensitization) and loses resistance to intergranular corrosion. 316L (C ≤ 0.030 %) avoids this and is the standard for welded parts, but has a lower minimum YS (170 vs. 205 MPa). That is why mills sell plate and pipe dual-certified 316/316L: L chemistry with 316 strength. 316H (C 0.04–0.10 % and coarse grain) is the opposite: high carbon for creep strength above ~540 °C. 316Ti ties up the carbon with titanium and is the preferred European equivalent (1.4571), while 316LN adds nitrogen to recover the strength lost to the low carbon.

Heat treatments required by the standards

Delivery conditions and temperatures
StandardDelivery conditionTemperature
ASTM A240, A479, A312, A213, A182 (316, 316L, 316N, 316LN) Solution annealed and rapidly cooled (water or other fast medium)≥ 1040 °C (1900 °F)
ASTM A213 / A312 / A240 316H Solution annealed, ASTM grain size No. 7 or coarser≥ 1040 °C (1900 °F)
ASTM 316Ti / EN 1.4571 Solution annealed; optional stabilizing treatment by agreement≥ 1040 °C; stabilizing ≈ 870–900 °C*
EN 10088-2/-3 (1.4401, 1.4404, 1.4435, 1.4571) Solution annealed (+AT), cooled in water or fast air1020–1120 °C*
ASTM A351 CF8M / CF3M Solution annealed and water quenched≥ 1040 °C (1900 °F)
ASTM F138 / ISO 5832-1 (316LVM) Annealed, cold worked or extra hard (by condition)per manufacturer

Plan an open-die forging in 316 / 316L stainless: reduction, slenderness and how much material to send →Simulate the cutting plan of the ingot or bar →

Variants in the family

Variants of 316 / 316L stainless
VariantStandardsDifferenceYS / UTS
316L (S31603, 1.4404) A240, A182 F316L, A312 TP316L, A403 WP316L, CF3MC ≤ 0.030 %: immune to sensitization in normal welding170 / 485 MPa (dual certified: 205 / 515)
316H (S31609) A240, A182 F316H, A312/A213 TP316H, A376C 0.04–0.10 % and coarse grain: creep above ~540 °C205 / 515 MPa
316Ti (S31635, 1.4571) A240, A182 F316Ti, A312 TP316Ti, EN 10088Ti 5×(C+N) to 0.70 % stabilizes the carbon205 / 515 MPa
316N / 316LN (S31651 / S31653, 1.4429) A240, A182 F316N/F316LN, A312 TP316LN, CF3MNN 0.10–0.16 % (EN up to 0.22 %): more strength and austenite stability, cryogenic use316LN 205 / 515; 316N 240 / 550 MPa
1.4435 (high Mo/Ni 316L) EN 10088, BN2 / 316L UG (urea)*Mo 2.5–3.0 %, Ni 12.5–15 %, minimal ferrite: pharmaceutical and urea220 / 520 MPa (plate)
316LVM (S31673, 1.4441) ASTM F138, F139, ISO 5832-1Vacuum remelted, Cr + 3.3 Mo ≥ 26, S ≤ 0.010, controlled inclusion cleanliness190 / 490 MPa annealed

Corrosion, PREN and temperature

  • PREN (Cr + 3.3 Mo + 16 N): ≈ 22.6 at the ASTM minimum and ≈ 25 typical for 316/316L; ≈ 26 for 1.4435 and 316LVM. Resists stagnant seawater only at low temperatures; for high chlorides use 904L, duplex or super austenitics.
  • Chloride stress corrosion cracking: significant risk above ~60 °C with chlorides and tensile stress, as in every Cr-Ni austenitic.
  • Sensitization: the ~425 to 815 °C range precipitates Cr carbides; prefer 316L or 316Ti in welded parts and check by ASTM A262 (practices A/E) or ISO 3651-2.
  • Sigma phase: long exposure between ~550 and 900 °C forms sigma and reduces toughness; more critical in 316 with ferrite (welds, CF8M).
  • Temperature: oxidation acceptable up to ~870 °C intermittent and ~925 °C continuous*; above ~540 °C use 316H (ASME only allows 316 stresses in that range with C ≥ 0.04 %). Good toughness in cryogenic service.
  • NACE MR0175/ISO 15156-3 and MR0103: accepted solution annealed, without cold work to increase strength, hardness ≤ 22 HRC (237 HBW), within the environmental limits of Table A.2 (≈ 60 °C and pH2S ≤ 100 kPa*).

Compare alloys by corrosive medium, concentration and temperature →

Implant grade 316LVM (ASTM F138 / ISO 5832-1)

  • Primary melting followed by vacuum arc remelting (VAR) or ESR for inclusion cleanliness, verified by ASTM E45*.
  • Narrower chemistry than 316L: Cr 17–19, Ni 13–15, Mo 2.25–3.00, P ≤ 0.025, S ≤ 0.010, Cu ≤ 0.50 and Cr + 3.3 Mo ≥ 26.0.
  • Fully austenitic microstructure, no delta ferrite, non-magnetic even after forming.
  • Supplied annealed, cold worked or extra hard; strength rises from ~490 MPa (annealed) to more than 1000 MPa in cold-worked wire/small bar.
  • Used in plates, bone screws, intramedullary nails, cerclage wire, stents and instruments; in Brazil, ABNT NBR ISO 5832-1.

Welding

Usual welding practice
ItemUsual practice
316 / 316L consumable ER316L or ER316LSi (AWS A5.9), E316L-16 (A5.4); EN ISO 14343 19 12 3 L (Si)
316H consumable ER316H / E316H-16 (C 0.04–0.08 %) to keep creep strength
316Ti consumable ER316L or ER318 (Nb stabilized)*; Ti does not transfer well across the arc
Cast CF8M / CF3M ER316 / ER316L; casting repair follows A351/A488
Preheat Not required
Interpass ≤ 150 °C (common practice; some specifications accept 175 °C)
Ferrite in the weld metal FN 3–10 to avoid hot cracking; low or none in cryogenic or urea service
PWHT Not required; solution annealing only if required for corrosion. Dissimilar joint with carbon steel: ER309LMo

Filler metal for welding

The wire composition is usually not identical to the material: each page explains why.

International equivalents

Equivalent designations
SystemDesignation
AISI / SAE 316, 316L, 316H, 316Ti, 316N, 316LN; SAE 30316 / 30316L
UNS S31600, S31603, S31609, S31635, S31651, S31653, S31673; castings J92900 (CF8M), J92800 (CF3M)
EN / W.Nr. 1.4401 X5CrNiMo17-12-2; 1.4404 X2CrNiMo17-12-2; 1.4436 X3CrNiMo17-13-3; 1.4435 X2CrNiMo18-14-3; 1.4571 X6CrNiMoTi17-12-2; 1.4429 X2CrNiMoN17-13-3; 1.4441 X2CrNiMo18-15-3; castings 1.4408 / 1.4409
ABNT NBR 5601: 316, 316L, 316N, 316Ti*; NBR ISO 5832-1 (implant)
JIS SUS316, SUS316L, SUS316H*, SUS316Ti, SUS316N, SUS316LN; cast SCS14A (CF8M), SCS16A (CF3M)
GB (China) 06Cr17Ni12Mo2 (316), 022Cr17Ni12Mo2 (316L), 07Cr17Ni12Mo2 (316H), 06Cr17Ni12Mo2Ti (316Ti), 022Cr17Ni12Mo2N (316LN)*
ISO / others ISO 15510 X2CrNiMo17-12-2; old AFNOR Z2CND17-12; BS 316S11 / 316S31*

Equivalence is approximate: EN limits Mo to 2.00–2.50 % in 1.4401/1.4404 and S to 0.015 %, and the mechanical minimums differ; check the order standard before substituting.

Typical applications

Form or industryWhere it is used
Chemicals and petrochemicals Piping, vessels, exchangers and tanks for organic acids, dilute sulfuric acid and media with moderate chlorides
Oil and gas and offshore Instrumentation tubing, fittings, F316L flanges, CF8M/CF3M valves, marine atmosphere
Food, beverage and pharmaceutical A270 sanitary tubing, tanks, reactors; low-ferrite 1.4435 in purified water lines
Pulp and paper, water treatment Bleaching, pumps, screens, effluent piping
High temperature and power 316H in superheaters, headers and steam piping; 316Ti in exhausts and exchangers
Cryogenics 316LN in tanks and components for liquefied gases and superconducting magnets
Medical 316LVM in orthopedic implants, screws, stents and surgical instruments

Frequently asked questions

Can I use 316L instead of 316?

Yes for corrosion, and it is preferred for welding. But the minimum YS of 316L is 170 MPa vs. 205 MPa; if the design was calculated with 316, order material dual-certified 316/316L.

What is the difference between F316L, TP316L, WP316L and CF3M?

It is the same alloy in different forms: F = forging (A182), TP = pipe/tube (A312/A213), WP = welding fitting (A403) and CF3M = casting (A351). The composition is almost the same; the casting has more Cr and Si and contains ferrite.

316Ti or 316L?

Both resist sensitization. 316L dominates the ASTM market; 316Ti (1.4571) is traditional in Europe and keeps a little more strength at temperature, but is harder to polish and to weld without Ti loss.

Is 316 magnetic?

Solution annealed it is practically non-magnetic. Cold work can form martensite and leave slight magnetism; welds and CF8M castings attract a little because of the ferrite. 316LVM is specified to remain non-magnetic.

Need 316 / 316L stainless?Bars, forgings and parts with EN 10204 3.1 certificate.

Forms and stock of 316 / 316L stainless

Dustre supplies 316 / 316L stainless as bar, plate, pipe and tube, forgings and flanges, fittings and castings, cut to size, with forged and machined parts to drawing (shafts, discs, rings and blocks) and a 3.1 certificate.

In stock in Osasco/SP, Brazil: plate from 5 mm, round bar from Ø 23 to 210 mm and tube from Ø 114.3 mm. List updated on 11/13/2026.

See the full ready-to-ship stock · Request a quote for 316 / 316L stainless

Where to buy 316 / 316L stainless in Brazil?

Dustre supplies 316 / 316L stainless as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

See also

HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp

We use your data only to answer this quote. Privacy. · WhatsApp +55 11 98649-0075 · Mon–Thu 07:00–17:00 · Fri 07:00–16:00 (Brasília time)