Incoloy 825 – UNS N08825

Titanium-stabilized nickel-iron-chromium alloy with molybdenum and copper

Download data sheet (PDF)

Ni-Fe-Cr alloy with Mo, Cu and Ti, developed for aqueous corrosion: sulfuric and phosphoric acids, chloride stress corrosion cracking and intergranular corrosion (Ti-stabilized). It is the reference material for sour-well tubing and pickling equipment. Pitting resistance is moderate (PREN ≈ 31).

Technical review Oct 2026 · minimum values per the cited standard; physical properties are typical; values marked * to be confirmed in the standard

FamilyNickel alloy
UNSN08825
W.Nr. / EN2.4858 – NiCr21Mo
PREN (Cr + 3.3Mo)≈ 31

Designations and equivalents

Designations of Incoloy 825 – UNS N08825
SystemDesignation
UNS N08825
W.Nr./EN 2.4858 – NiCr21Mo
DIN NiCr21Mo
JIS NCF 825
Trade names Incoloy 825 (Special Metals), Nicrofer 4221 (VDM), Alloy 825
Others ISO NiFe30Cr21Mo3

Standards by product form

Standards for Incoloy 825 – UNS N08825
FormStandard
Bar ASTM B425
Forging ASTM B564
Plate ASTM B424
Tube ASTM B423 (seamless), B163, B705 (welded)

Tolerances and HS codes

  • Forged bars (round and square): machining allowance from 2 mm (Ø 6–16 mm) to 24 mm (Ø 400–500 mm) on the diameter. E.g. Ø 100–125 mm finished: +7 mm, tolerance +6 / −0 (length up to 3,500 mm).
  • Forged discs: allowance of 4 to 9 mm on the diameter and 3 to 11 mm on the height, plus-only tolerance.
  • Cutting and machining: band saw −0 / +5 to +15 mm on length; waterjet +10 % of thickness on the diameter (min. 2 mm); machined parts −0 / +2 to +5 mm on the diameter. See the full tables (INF 002 and INF 003, the same for every alloy).
Tariff classification of Incoloy 825: NCM, HS, HTS and CN by product form
FormNCM (Brazil, 8 digits)HS (international, 6 digits)HTS (USA, 10 digits)*CN (European Union, 8 digits)*
Forged bar7505.12.107505.127505.12.30007505 12 00
Hot-rolled bar7505.12.107505.127505.12.30007505 12 00
Plate (> 10 mm, width ≥ 600 mm)7506.20.007506.207506.20.30007506 20 00
Seamless pipe7507.12.007507.127507.12.00007507 12 00
Welded pipe7507.12.007507.127507.12.00007507 12 00
Flange and fitting7507.20.007507.207507.20.00007507 20 00

Tariff class: nickel alloy (by chemical composition, under the Chapter 72 Notes and Section XV Note 5).

*: US and EU codes for reference. NCM per current legislation (General Rules of Interpretation, Notes to Chapters 72, 74 and 75 and Section XV Note 5). Confirm the final code with your customs broker according to the item size and finish. HS = first 6 digits of the NCM.

Chemical composition (%)

ASTM B425 / B564 (UNS N08825)

Chemical composition of Incoloy 825 – UNS N08825, per ASTM B425 / B564 (UNS N08825)
ElementRange (%)
Ni 38.0 – 46.0
Fe ≥ 22.0
Cr 19.5 – 23.5
Mo 2.5 – 3.5
Cu 1.5 – 3.0
Ti 0.6 – 1.2
C ≤ 0.05
Mn ≤ 1.0
Si ≤ 0.5
Al ≤ 0.2
S ≤ 0.03

Calculate the PREN of Incoloy 825 in the PREN calculator →

Mechanical properties

annealed (ASTM B564 / B425)

Mechanical properties of Incoloy 825 – UNS N08825
PropertyValue
Yield strength (0.2%) ≥ 241 MPa
Tensile strength ≥ 586 MPa
Elongation ≥ 30%

Typical physical properties

Typical values at 20 °C
PropertyValue
Density 8.14 g/cm³
Melting range 1,370 – 1,400 °C
Modulus of elasticity 196 GPa
Thermal conductivity (20 °C) 11.1 W/m·K
Thermal expansion (20–100 °C) 14.0 µm/m·K
Electrical resistivity 113 µΩ·cm

Calculate the weight of Incoloy 825 bar, plate or pipe →

Heat treatment, welding and machining

ItemUsual practice
Service temperature From cryogenic up to ~540 °C (usual limit in ASME pressure vessels). Not indicated for creep service.
Heat treatment Stabilizing anneal at ≈ 940 °C (range 920 – 980 °C), with rapid cooling. Forms Ti carbides and prevents sensitization. Not age hardenable.
Welding Good weldability. Most used consumable: AWS ERNiCrMo-3 / ENiCrMo-3 (625, over-alloyed); alternative ERNiFeCr-1 (FM 65 type).
Machining Similar to high-alloy austenitic stainless: work hardens; use carbide, moderate speed and coolant.

Plan an open-die forging in Incoloy 825: reduction, slenderness and how much material to send →Simulate the cutting plan of the ingot or bar →

Filler metal for welding

The wire composition is usually not identical to the material: each page explains why.

Typical applications

  • Well tubing and components with H₂S/CO₂ (oil and gas)
  • Sulfuric and phosphoric acid equipment
  • Pickling tanks, baskets and coils
  • Gas scrubbers (FGD)
  • Heat exchangers cooled with brackish water
  • Nuclear fuel reprocessing

Alternatives: 904L or Alloy 20 (N08020) in sulfuric acid at lower cost; 625, C276 or 6Mo super-austenitic when there is a risk of pitting or crevice corrosion in chlorides; 28 (N08028) as a similar option.

Compare alloys by corrosive medium, concentration and temperature →

Incoloy 825: complete guide

What Incoloy 825 is

Incoloy 825 belongs to the family of nickel alloys, in the nickel-iron-chromium group for aqueous corrosion. It derives from Incoloy 800 by adding molybdenum, copper and titanium and increasing the nickel: molybdenum gives resistance to pitting and reducing media, copper protects in sulfuric acid, titanium stabilizes the alloy against intergranular corrosion and the high nickel makes it practically immune to chloride stress corrosion cracking.

Mechanical properties

Annealed, ASTM B425 requires a minimum yield strength of 241 MPa, minimum tensile strength of 586 MPa and minimum elongation of 30%. The alloy does not harden by heat treatment.

Corrosion and limits of use

825 resists sulfuric and phosphoric acid over a wide concentration range, organic acids, moderate chlorides and stress corrosion cracking, with a PREN of 28 to 35, and is qualified by NACE MR0175 for H2S wells. It is limited in hydrochloric acid and in crevices in stagnant seawater, where Inconel 625 or C-276 are indicated.

Applications

Sulfuric and phosphoric acid tanks, heat exchangers and piping, pickling equipment, production tubing and oil and gas well components in sour service, desulfurization absorbers, nuclear fuel reprocessing equipment and valve and pump components for the chemical industry. Alternatives: Alloy 20 for sulfuric acid and Alloy 28 (UNS N08028) for phosphoric acid and wells.

Supply forms and Dustre services

Round bars and blocks forged in open die, cut to size on a band saw, with rough or finish machining, solution annealing or annealing in our own furnaces and hardness, tensile and impact testing. All material is supplied with a 3.1 inspection certificate and heat traceability.

Frequently asked questions

What is the chemical composition of Incoloy 825?

Per ASTM B425 / B564 (UNS N08825): Ni 38.0 – 46.0; Fe ≥ 22.0; Cr 19.5 – 23.5; Mo 2.5 – 3.5; Cu 1.5 – 3.0; Ti 0.6 – 1.2.

Which standards cover Incoloy 825?

Bar: ASTM B425. Forging: ASTM B564. Plate: ASTM B424. Tube: ASTM B423 (seamless), B163, B705 (welded).

Up to what temperature can Incoloy 825 be used?

From cryogenic up to ~540 °C (usual limit in ASME pressure vessels). Not indicated for creep service.

Which materials can replace Incoloy 825?

904L or Alloy 20 (N08020) in sulfuric acid at lower cost; 625, C276 or 6Mo super-austenitic when there is a risk of pitting or crevice corrosion in chlorides; 28 (N08028) as a similar option.

Where to buy Incoloy 825 in Brazil?

Dustre supplies Incoloy 825 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

Need Incoloy 825?Bars, forgings and parts with EN 10204 3.1 certificate.

Forms and stock of Incoloy 825

Dustre supplies Incoloy 825 as bar, plate, pipe and tube and forgings and flanges, cut to size, with forged and machined parts to drawing (shafts, discs, rings and blocks) and a 3.1 certificate.

Not in stock at the moment: supplied to order, with lead time in the quotation.

See the full ready-to-ship stock · Request a quote for Incoloy 825

Where to buy Incoloy 825 in Brazil?

Dustre supplies Incoloy 825 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

See also

HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp

We use your data only to answer this quote. Privacy. · WhatsApp +55 11 98649-0075 · Mon–Thu 07:00–17:00 · Fri 07:00–16:00 (Brasília time)