Nickel 200 – UNS N02200
Commercially pure nickel (≥ 99.0% Ni)
Commercially pure wrought nickel, with high thermal and electrical conductivity and excellent resistance to caustic soda and other alkalis, neutral salts and dry fluorine. It is ferromagnetic. Limited to ~315 °C: above that, carbon precipitates as graphite at the grain boundaries, and Nickel 201 (low C) must be used.
Designations and equivalents
| System | Designation |
|---|---|
| UNS | N02200 |
| W.Nr./EN | 2.4066 – Ni 99.2 |
| DIN | Ni99.2 |
| JIS | NW2200 |
| Trade names | Nickel 200 (Special Metals), VDM Nickel 200, Alloy 200 |
| Others | Nickel 201: UNS N02201 / 2.4068 (C ≤ 0.02) |
Standards by product form
| Form | Standard |
|---|---|
| Bar | ASTM B160 |
| Forging | ASTM B564 |
| Plate | ASTM B162 |
| Tube | ASTM B161 (seamless), B163 (exchanger) |
Tolerances and HS codes
- Forged bars (round and square): machining allowance from 2 mm (Ø 6–16 mm) to 24 mm (Ø 400–500 mm) on the diameter. E.g. Ø 100–125 mm finished: +7 mm, tolerance +6 / −0 (length up to 3,500 mm).
- Forged discs: allowance of 4 to 9 mm on the diameter and 3 to 11 mm on the height, plus-only tolerance.
- Cutting and machining: band saw −0 / +5 to +15 mm on length; waterjet +10 % of thickness on the diameter (min. 2 mm); machined parts −0 / +2 to +5 mm on the diameter. See the full tables (INF 002 and INF 003, the same for every alloy).
| Form | NCM (Brazil, 8 digits) | HS (international, 6 digits) | HTS (USA, 10 digits)* | CN (European Union, 8 digits)* |
|---|---|---|---|---|
| Forged bar | 7505.11.10 | 7505.11 | 7505.11.3000 | 7505 11 00 |
| Hot-rolled bar | 7505.11.10 | 7505.11 | 7505.11.3000 | 7505 11 00 |
| Plate (> 10 mm, width ≥ 600 mm) | 7506.10.00 | 7506.10 | 7506.10.3000 | 7506 10 00 |
| Seamless pipe | 7507.11.00 | 7507.11 | 7507.11.0000 | 7507 11 00 |
| Welded pipe | 7507.11.00 | 7507.11 | 7507.11.0000 | 7507 11 00 |
| Flange and fitting | 7507.20.00 | 7507.20 | 7507.20.0000 | 7507 20 00 |
Tariff class: unalloyed nickel (by chemical composition, under the Chapter 72 Notes and Section XV Note 5).
*: US and EU codes for reference. NCM per current legislation (General Rules of Interpretation, Notes to Chapters 72, 74 and 75 and Section XV Note 5). Confirm the final code with your customs broker according to the item size and finish. HS = first 6 digits of the NCM.
Chemical composition (%)
ASTM B160 / B564 (UNS N02200)
| Element | Range (%) |
|---|---|
| Ni | ≥ 99.0 |
| Cu | ≤ 0.25 |
| Fe | ≤ 0.40 |
| Mn | ≤ 0.35 |
| C | ≤ 0.15 |
| Si | ≤ 0.35 |
| S | ≤ 0.01 |
Mechanical properties
annealed (ASTM B564 / B160)
| Property | Value |
|---|---|
| Yield strength (0.2%) | ≥ 105 MPa |
| Tensile strength | ≥ 380 MPa |
| Elongation | ≥ 40% |
| Hot rolled (B160): YS / UTS / El. | ≥ 105 MPa / ≥ 415 MPa / ≥ 35% |
Typical physical properties
| Property | Value |
|---|---|
| Density | 8.89 g/cm³ |
| Melting range | 1,435 – 1,446 °C |
| Modulus of elasticity | 204 GPa |
| Thermal conductivity (20 °C) | 70.2 W/m·K |
| Thermal expansion (20–100 °C) | 13.3 µm/m·K |
| Electrical resistivity | 9.5 µΩ·cm |
Heat treatment, welding and machining
| Item | Usual practice |
|---|---|
| Service temperature | Up to ~315 °C. Above that, use Nickel 201 (risk of intergranular graphitization). |
| Heat treatment | Annealing at ≈ 705 – 870 °C, controlling time and temperature to avoid grain growth. Air or water cooling. Not hardenable by heat treatment. |
| Welding | Good weldability. Consumables: AWS A5.14 ERNi-1 (FM 61 type) and AWS A5.11 ENi-1 (141 type). Rigorous cleaning: sulfur and lead cause cracking. |
| Machining | 'Gummy' material in the annealed condition; machines better in the cold-worked condition. Use a sharp, positive-rake tool. |
Plan an open-die forging in Nickel 200: reduction, slenderness and how much material to send →Simulate the cutting plan of the ingot or bar →
Filler metal for welding
The wire composition is usually not identical to the material: each page explains why.
Typical applications
- Evaporators and piping for caustic soda (NaOH)
- Food and synthetic fiber processing
- Handling of fluorine and anhydrous HF
- Electronic components, terminals and batteries
- Anodes and cathodes in electrolysis
- Tanks for chemical transport
Alternatives: Nickel 201 above 315 °C or in hot concentrated caustic soda; Monel 400 for seawater and HF with more mechanical strength; Inconel 600 when sulfur or hot oxidation is present.
Compare alloys by corrosive medium, concentration and temperature →
Nickel 200: complete guide
What Nickel 200 is
Nickel 200 belongs to the family of nickel alloys as its simplest member: commercially pure nickel, with at least 99% nickel and small amounts of carbon, manganese, iron, silicon and copper. It is ductile, tough, ferromagnetic up to about 360 °C and hardens only by cold work. Its valuable property is resistance to caustic soda and fluorine, which no more highly alloyed grade matches.
Nickel 200 and Nickel 201
The carbon of up to 0.15% in Nickel 200 precipitates as graphite in prolonged exposures above about 315 °C, embrittling the material; that is why the use of 200 is limited to that temperature. For service above 315 °C, Nickel 201 is specified, with carbon up to 0.02%; commercial material is usually dual certified 200 / 201.
Corrosion and limits of use
Nickel 200 resists sodium and potassium hydroxide in all concentrations, including molten, fluorine, anhydrous hydrofluoric acid and fluorides, neutral and reducing media, fresh water and flowing seawater. It is limited in oxidizing media such as nitric acid and ferric chloride, in stagnant seawater and in aerated ammoniacal solutions. For seawater and aqueous hydrofluoric acid, Monel 400 is the usual choice; when sulfur or hot oxidation is present, Inconel 600.
Applications
Caustic soda and potash evaporators, tanks and piping, reactors and equipment for fluorine and fluoride production, synthetic fiber production components, food processing equipment, electronic and electrochemical components, and aerospace and defense parts that require pure nickel.
Supply forms and Dustre services
Round bars and blocks forged in open die, cut to size on a band saw, with rough or finish machining, solution annealing or annealing in our own furnaces and hardness, tensile and impact testing. All material is supplied with a 3.1 inspection certificate and heat traceability.
Frequently asked questions
What is the chemical composition of Nickel 200?
Per ASTM B160 / B564 (UNS N02200): Ni ≥ 99.0; Cu ≤ 0.25; Fe ≤ 0.40; Mn ≤ 0.35; C ≤ 0.15; Si ≤ 0.35.
Which standards cover Nickel 200?
Bar: ASTM B160. Forging: ASTM B564. Plate: ASTM B162. Tube: ASTM B161 (seamless), B163 (exchanger).
Up to what temperature can Nickel 200 be used?
Up to ~315 °C. Above that, use Nickel 201 (risk of intergranular graphitization).
Which materials can replace Nickel 200?
Nickel 201 above 315 °C or in hot concentrated caustic soda; Monel 400 for seawater and HF with more mechanical strength; Inconel 600 when sulfur or hot oxidation is present.
Where to buy Nickel 200 in Brazil?
Dustre supplies Nickel 200 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.