Dustre
EN
Customer area

Incoloy 800HT – UNS N08811

Iron-nickel-chromium alloy for creep and oxidation at high temperature

Download data sheet (PDF)

Fe-Ni-Cr alloy of the 800 family with controlled carbon (0.06 – 0.10%), Al+Ti of 0.85 to 1.20% and a coarse grain obtained by solution annealing above 1,150 °C. This combination gives the highest creep and rupture strength of the family. It resists oxidation and carburization. Usually supplied dual certified 800H/800HT. By composition (Fe ≥ 39.5%) it is also classified as a high-alloy austenitic stainless.

Technical review Oct 2026 · minimum values per the cited standard; physical properties are typical; values marked * to be confirmed in the standard

FamilyNickel alloy
UNSN08811 (800H: N08810; 800: N08800)
W.Nr. / EN1.4959 – X8NiCrAlTi32-21 (800H: 1.4958)

Designations and equivalents

Designations of Incoloy 800HT – UNS N08811
SystemDesignation
UNS N08811 (800H: N08810; 800: N08800)
W.Nr./EN 1.4959 – X8NiCrAlTi32-21 (800H: 1.4958)
DIN X8NiCrAlTi32-21
JIS NCF 800HT
Trade names Incoloy 800HT (Special Metals), Nicrofer 3220 HP (VDM), Alloy 800HT
Others Dual certification 800H/800HT

Standards by product form

Standards for Incoloy 800HT – UNS N08811
FormStandard
Bar ASTM B408
Forging ASTM B564
Plate ASTM B409; ASTM A240
Tube ASTM B407 (seamless), B163 (exchanger), B514/B515 (welded)

Tolerances and HS codes

  • Forged bars (round and square): machining allowance from 2 mm (Ø 6–16 mm) to 24 mm (Ø 400–500 mm) on the diameter. E.g. Ø 100–125 mm finished: +7 mm, tolerance +6 / −0 (length up to 3,500 mm).
  • Forged discs: allowance of 4 to 9 mm on the diameter and 3 to 11 mm on the height, plus-only tolerance.
  • Cutting and machining: band saw −0 / +5 to +15 mm on length; waterjet +10 % of thickness on the diameter (min. 2 mm); machined parts −0 / +2 to +5 mm on the diameter. See the full tables (INF 002 and INF 003, the same for every alloy).
Tariff classification of Incoloy 800HT: NCM, HS, HTS and CN by product form
FormNCM (Brazil, 8 digits)HS (international, 6 digits)HTS (USA, 10 digits)*CN (European Union, 8 digits)*
Forged bar7222.30.007222.307222.30.00247222 30 51
Hot-rolled bar7222.11.007222.117222.11.00597222 11 11
Plate (> 10 mm, width ≥ 600 mm)7219.21.007219.217219.21.00207219 21 10
Seamless pipe7304.41.907304.417304.41.60457304 41 00
Welded pipe7306.40.007306.407306.40.50857306 40 80
Flange and fitting7307.21.007307.217307.21.50007307 21 00

Tariff class: stainless steel (by chemical composition, under the Chapter 72 Notes and Section XV Note 5). Fe-Ni-Cr alloy in which iron predominates by weight: under Section XV Note 5 and Chapter 72 Note 1(e) it is classified as stainless steel (7219, 7222, 7304), not as a Chapter 75 nickel alloy.

*: US and EU codes for reference. NCM per current legislation (General Rules of Interpretation, Notes to Chapters 72, 74 and 75 and Section XV Note 5). Confirm the final code with your customs broker according to the item size and finish. HS = first 6 digits of the NCM.

Chemical composition (%)

ASTM B408 / B564 (UNS N08811)

Chemical composition of Incoloy 800HT – UNS N08811, per ASTM B408 / B564 (UNS N08811)
ElementRange (%)
Ni 30.0 – 35.0
Cr 19.0 – 23.0
Fe ≥ 39.5
C 0.06 – 0.10
Al 0.25 – 0.60
Ti 0.25 – 0.60
Al + Ti 0.85 – 1.20
Mn ≤ 1.50
Si ≤ 1.0
Cu ≤ 0.75
S ≤ 0.015

Calculate the PREN of Incoloy 800HT in the PREN calculator →

Mechanical properties

solution annealed (ASTM B564 / B408)

Mechanical properties of Incoloy 800HT – UNS N08811
PropertyValue
Yield strength (0.2%) ≥ 172 MPa
Tensile strength ≥ 448 MPa
Elongation ≥ 30%
Grain size ASTM No. 5 or coarser

Typical physical properties

Typical values at 20 °C
PropertyValue
Density 7.94 g/cm³
Melting range 1,357 – 1,385 °C
Modulus of elasticity 196 GPa
Thermal conductivity (20 °C) 11.5 W/m·K
Thermal expansion (20–100 °C) 14.4 µm/m·K

Calculate the weight of Incoloy 800HT bar, plate or pipe →

Heat treatment, welding and machining

ItemUsual practice
Service temperature Designed for creep above ~600 °C, up to 899 °C per ASME (II-D) and up to ~1,000 °C per European standards (EN/VdTÜV); oxidation and carburization resistance up to ~1,100 °C. Below ~600 °C the plain 800 alloy (N08800) is adequate.
Heat treatment Solution annealing at ≥ 1,149 °C (usual range 1,150 – 1,200 °C) until ASTM grain size No. 5 or coarser is reached, with rapid cooling. Not age hardenable.
Welding Up to ~790 °C: AWS ERNiCr-3 (FM 82) and ENiCrFe-2 (Inco-Weld A type). Above ~790 °C: ERNiCrCoMo-1 (FM 617) and ENiCrCoMo-1 (electrode 117).
Machining Comparable to high-alloy austenitic stainless: work hardens; use carbide, positive feed and coolant.

Plan an open-die forging in Incoloy 800HT: reduction, slenderness and how much material to send →Simulate the cutting plan of the ingot or bar →

Filler metal for welding

The wire composition is usually not identical to the material: each page explains why.

Typical applications

  • Steam reformer pigtails and headers (hydrogen, ammonia, methanol)
  • Superheaters and reheaters
  • High-temperature heat exchangers
  • Muffles, retorts and baskets for heat treatment furnaces
  • Petrochemical and cracking furnaces
  • Carburizing and nitriding furnace components

Alternatives: Incoloy 800 (N08800) below ~600 °C, with no creep requirement; Inconel 600/601 for nitriding or severe cyclic oxidation; Inconel 617 when more creep resistance is needed; 310/253MA stainless as a lower-cost option.

Compare alloys by corrosive medium, concentration and temperature →

Incoloy 800HT: complete guide

What Incoloy 800HT is

Incoloy 800HT belongs to the family of nickel alloys, in the iron-nickel-chromium group for high temperature. It is the version of Incoloy 800 with the highest creep resistance: carbon controlled between 0.06 and 0.10%, the sum of aluminum and titanium between 0.85 and 1.20% and high-temperature solution annealing, which produces ASTM grain size 5 or coarser, raise the allowable stresses above 600 °C.

800, 800H and 800HT

800 (N08800) is the basic, annealed alloy, for use up to about 600 °C. 800H (N08810) adds carbon of 0.05 to 0.10% and a coarse grain, and 800HT (N08811) further adds control of Al + Ti, with the highest creep values. For creep design, 800H or 800HT must be specified.

Mechanical properties

Solution annealed, ASTM B408 requires a minimum yield strength of 172 MPa, minimum tensile strength of 448 MPa, minimum elongation of 30% and ASTM grain size 5 or coarser. The room-temperature minimums are lower than those of annealed 800 precisely because of the coarse grain; the alloy's advantage lies in the creep allowable stresses given by the design code.

Corrosion and limits of use

800HT resists oxidation in air up to about 1,100 °C and has good resistance to carburization, moderate nitriding and sulfidation, in the latter superior to high-nickel alloys such as Inconel 600. In aqueous corrosion it behaves like a high-nickel austenitic, with good stress corrosion resistance. Use under load is defined by the creep stresses of the design standard, up to 899 °C per ASME and up to about 1,000 °C per European standards.

Applications

Tubes and headers of hydrogen and ammonia reforming furnaces and ethylene pyrolysis, radiant tubes, heat exchangers and superheaters, heat treatment furnace components, retorts, supports and grids, and power generation and high-temperature chemical process equipment. For less severe creep, 310S; for severe carburization, Inconel 601.

Supply forms and Dustre services

Round bars and blocks forged in open die, cut to size on a band saw, with rough or finish machining, solution annealing or annealing in our own furnaces and hardness, tensile and impact testing. All material is supplied with a 3.1 inspection certificate and heat traceability.

Frequently asked questions

What is the chemical composition of Incoloy 800HT?

Per ASTM B408 / B564 (UNS N08811): Ni 30.0 – 35.0; Cr 19.0 – 23.0; Fe ≥ 39.5; C 0.06 – 0.10; Al 0.25 – 0.60; Ti 0.25 – 0.60.

Which standards cover Incoloy 800HT?

Bar: ASTM B408. Forging: ASTM B564. Plate: ASTM B409; ASTM A240. Tube: ASTM B407 (seamless), B163 (exchanger), B514/B515 (welded).

Up to what temperature can Incoloy 800HT be used?

Designed for creep above ~600 °C, up to 899 °C per ASME (II-D) and up to ~1,000 °C per European standards (EN/VdTÜV); oxidation and carburization resistance up to ~1,100 °C. Below ~600 °C the plain 800 alloy (N08800) is adequate.

Which materials can replace Incoloy 800HT?

Incoloy 800 (N08800) below ~600 °C, with no creep requirement; Inconel 600/601 for nitriding or severe cyclic oxidation; Inconel 617 when more creep resistance is needed; 310/253MA stainless as a lower-cost option.

Where to buy Incoloy 800HT in Brazil?

Dustre supplies Incoloy 800HT as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

Need Incoloy 800HT?Bars, forgings and parts with EN 10204 3.1 certificate.

Forms and stock of Incoloy 800HT

Dustre supplies Incoloy 800HT as bar, plate, pipe and tube and forgings and flanges, cut to size, with forged and machined parts to drawing (shafts, discs, rings and blocks) and a 3.1 certificate.

Not in stock at the moment: supplied to order, with lead time in the quotation.

See the full ready-to-ship stock · Request a quote for Incoloy 800HT

Where to buy Incoloy 800HT in Brazil?

Dustre supplies Incoloy 800HT as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

See also

HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp

We use your data only to answer this quote. Privacy. · WhatsApp +55 11 98649-0075 · Mon–Thu 07:00–17:00 · Fri 07:00–16:00 (Brasília time)