Hastelloy C-4 – UNS N06455

Nickel-chromium-molybdenum alloy with high thermal stability

Download data sheet (PDF)

Ni-Cr-Mo alloy (16Cr-16Mo) with very low C and Si, stabilized with Ti and free of tungsten. This keeps it stable even after exposure to 650 – 1,040 °C: intergranular corrosion in the HAZ is minimal and ductility is retained, even in welded parts without PWHT. Corrosion resistance similar to C276 in reducing and oxidizing chloride media.

Technical review Oct 2026 · minimum values per the cited standard; physical properties are typical; values marked * to be confirmed in the standard

FamilyNickel alloy
UNSN06455
W.Nr. / EN2.4610 – NiMo16Cr16Ti
PREN (Cr + 3.3Mo, indicative)≈ 67

Designations and equivalents

Designations of Hastelloy C-4 – UNS N06455
SystemDesignation
UNS N06455
W.Nr./EN 2.4610 – NiMo16Cr16Ti
DIN NiMo16Cr16Ti
JIS NW6455
Trade names Hastelloy C-4 (Haynes), Nicrofer 6616 hMo (VDM), Alloy C4

Standards by product form

Standards for Hastelloy C-4 – UNS N06455
FormStandard
Bar ASTM B574
Forging ASTM B574 (forged bar); B564 does not cover N06455
Plate ASTM B575
Tube ASTM B622 (seamless), B619/B626 (welded)

Tolerances and HS codes

  • Forged bars (round and square): machining allowance from 2 mm (Ø 6–16 mm) to 24 mm (Ø 400–500 mm) on the diameter. E.g. Ø 100–125 mm finished: +7 mm, tolerance +6 / −0 (length up to 3,500 mm).
  • Forged discs: allowance of 4 to 9 mm on the diameter and 3 to 11 mm on the height, plus-only tolerance.
  • Cutting and machining: band saw −0 / +5 to +15 mm on length; waterjet +10 % of thickness on the diameter (min. 2 mm); machined parts −0 / +2 to +5 mm on the diameter. See the full tables (INF 002 and INF 003, the same for every alloy).
Tariff classification of Hastelloy C-4: NCM, HS, HTS and CN by product form
FormNCM (Brazil, 8 digits)HS (international, 6 digits)HTS (USA, 10 digits)*CN (European Union, 8 digits)*
Forged bar7505.12.107505.127505.12.30007505 12 00
Hot-rolled bar7505.12.107505.127505.12.30007505 12 00
Plate (> 10 mm, width ≥ 600 mm)7506.20.007506.207506.20.30007506 20 00
Seamless pipe7507.12.007507.127507.12.00007507 12 00
Welded pipe7507.12.007507.127507.12.00007507 12 00
Flange and fitting7507.20.007507.207507.20.00007507 20 00

Tariff class: nickel alloy (by chemical composition, under the Chapter 72 Notes and Section XV Note 5).

*: US and EU codes for reference. NCM per current legislation (General Rules of Interpretation, Notes to Chapters 72, 74 and 75 and Section XV Note 5). Confirm the final code with your customs broker according to the item size and finish. HS = first 6 digits of the NCM.

Chemical composition (%)

ASTM B574 / B575 (UNS N06455)

Chemical composition of Hastelloy C-4 – UNS N06455, per ASTM B574 / B575 (UNS N06455)
ElementRange (%)
Ni balance (≈ 65)
Cr 14.0 – 18.0
Mo 14.0 – 17.0
Fe ≤ 3.0
Co ≤ 2.0
Ti ≤ 0.70
Mn ≤ 1.0
Si ≤ 0.08
C ≤ 0.015
P ≤ 0.04
S ≤ 0.03

Calculate the PREN of Hastelloy C-4 in the PREN calculator →

Mechanical properties

solution annealed (ASTM B574)

Mechanical properties of Hastelloy C-4 – UNS N06455
PropertyValue
Yield strength (0.2%) ≥ 276 MPa
Tensile strength ≥ 690 MPa
Elongation ≥ 40%

Typical physical properties

Typical values at 20 °C
PropertyValue
Density 8.64 g/cm³
Melting range 1,335 – 1,380 °C
Modulus of elasticity 211 GPa (typical)
Thermal conductivity (20 °C) 10.1 W/m·K
Thermal expansion (20–100 °C) 10.8 µm/m·K

Calculate the weight of Hastelloy C-4 bar, plate or pipe →

Heat treatment, welding and machining

ItemUsual practice
Service temperature An alloy for aqueous corrosion. Its strength is keeping ductility and corrosion resistance after thermal exposure between 650 and 1,040 °C, not structural use at high temperature.
Heat treatment Solution annealing at ≈ 1,065 °C with rapid cooling (water). Normally used as welded, without PWHT.
Welding Good weldability. Consumables: AWS A5.14 ERNiCrMo-7 and AWS A5.11 ENiCrMo-7. Low heat input and interpass ≤ 100 °C (typical).
Machining Difficult, like the other Ni-Cr-Mo alloys: carbide, low speed and abundant coolant.

Plan an open-die forging in Hastelloy C-4: reduction, slenderness and how much material to send →Simulate the cutting plan of the ingot or bar →

Filler metal for welding

The wire composition is usually not identical to the material: each page explains why.

Typical applications

  • Reactors, exchangers and columns with chloride-contaminated acids
  • Pickling and acid regeneration
  • Flue gas desulfurization (FGD)
  • Pulp and paper bleaching
  • Pharmaceutical and agrochemical industry
  • Waste and effluent treatment

Alternatives: C276 in strongly reducing media, with greater availability; C22 or 59 when strong oxidizers are present.

Compare alloys by corrosive medium, concentration and temperature →

Hastelloy C-4: complete guide

What Hastelloy C-4 is

Hastelloy C-4 belongs to the family of nickel alloys, in the nickel-chromium-molybdenum group. Compared with C-276, it eliminates tungsten and limits iron to 3% max., which gives it thermal stability: it can be heated between 650 and 1,040 °C, for example when welding thick sections, without precipitating the phases that reduce corrosion resistance.

Mechanical properties

Solution annealed, ASTM B574 requires a minimum yield strength of 276 MPa, minimum tensile strength of 690 MPa and minimum elongation of 40%. The alloy is not hardenable by heat treatment.

Corrosion and limits of use

Resistance is similar to C-276 in dilute hydrochloric and sulfuric acid, chlorides, wet chlorine, organic acids and mixtures, with immunity to pitting, crevice corrosion and chloride stress corrosion cracking. In strongly oxidizing media C-22 is superior, and in hot concentrated hydrochloric acid B-2. It is an aqueous-corrosion alloy, used under the ASME code up to about 425 °C.

Applications

Welded reactors, exchangers, columns and piping in the chemical and pharmaceutical industry, chlor-alkali and wet chlorine process equipment, valve and pump components in chlorides, and pollution control equipment where the weld cannot be heat treated.

Supply forms and Dustre services

Round bars and blocks forged in open die, cut to size on a band saw, with rough or finish machining, solution annealing or annealing in our own furnaces and hardness, tensile and impact testing. All material is supplied with a 3.1 inspection certificate and heat traceability.

Frequently asked questions

What is the chemical composition of Hastelloy C-4?

Per ASTM B574 / B575 (UNS N06455): Ni balance (≈ 65); Cr 14.0 – 18.0; Mo 14.0 – 17.0; Fe ≤ 3.0; Co ≤ 2.0; Ti ≤ 0.70.

Which standards cover Hastelloy C-4?

Bar: ASTM B574. Forging: ASTM B574 (forged bar); B564 does not cover N06455. Plate: ASTM B575. Tube: ASTM B622 (seamless), B619/B626 (welded).

Up to what temperature can Hastelloy C-4 be used?

An alloy for aqueous corrosion. Its strength is keeping ductility and corrosion resistance after thermal exposure between 650 and 1,040 °C, not structural use at high temperature.

Which materials can replace Hastelloy C-4?

C276 in strongly reducing media, with greater availability; C22 or 59 when strong oxidizers are present.

Where to buy Hastelloy C-4 in Brazil?

Dustre supplies Hastelloy C-4 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

Need Hastelloy C-4?Bars, forgings and parts with EN 10204 3.1 certificate.

Forms and stock of Hastelloy C-4

Dustre supplies Hastelloy C-4 as bar, plate, pipe and tube and forgings and flanges, cut to size, with forged and machined parts to drawing (shafts, discs, rings and blocks) and a 3.1 certificate.

Not in stock at the moment: supplied to order, with lead time in the quotation.

See the full ready-to-ship stock · Request a quote for Hastelloy C-4

Where to buy Hastelloy C-4 in Brazil?

Dustre supplies Hastelloy C-4 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

See also

HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp

We use your data only to answer this quote. Privacy. · WhatsApp +55 11 98649-0075 · Mon–Thu 07:00–17:00 · Fri 07:00–16:00 (Brasília time)