Hastelloy C-22 – UNS N06022

Versatile nickel-chromium-molybdenum-tungsten alloy

Download data sheet (PDF)

Ni-Cr-Mo-W alloy with ~21% Cr, 13.5% Mo and 3% W. It resists oxidizing media (Cr) and reducing media (Mo and W) and mixed environments such as wet chlorine, ferric/cupric chloride and nitric + hydrochloric acids. It has pitting and crevice resistance superior to C276 and 625. Its consumable is the most used as an 'over-alloyed' filler for welding other alloys.

Technical review Oct 2026 · minimum values per the cited standard; physical properties are typical; values marked * to be confirmed in the standard

FamilyNickel alloy
UNSN06022
W.Nr. / EN2.4602 – NiCr21Mo14W
PREN (Cr + 3.3(Mo + 0.5W), indicative)≈ 70

Designations and equivalents

Designations of Hastelloy C-22 – UNS N06022
SystemDesignation
UNS N06022
W.Nr./EN 2.4602 – NiCr21Mo14W
DIN NiCr21Mo14W
JIS NW6022
Trade names Hastelloy C-22 (Haynes), Nicrofer 5621 hMoW (VDM), Inconel 622 (Special Metals), Alloy 22

Standards by product form

Standards for Hastelloy C-22 – UNS N06022
FormStandard
Bar ASTM B574
Forging ASTM B564; B462 (flanges and fittings)
Plate ASTM B575
Tube ASTM B622 (seamless), B619/B626 (welded)

Tolerances and HS codes

  • Forged bars (round and square): machining allowance from 2 mm (Ø 6–16 mm) to 24 mm (Ø 400–500 mm) on the diameter. E.g. Ø 100–125 mm finished: +7 mm, tolerance +6 / −0 (length up to 3,500 mm).
  • Forged discs: allowance of 4 to 9 mm on the diameter and 3 to 11 mm on the height, plus-only tolerance.
  • Cutting and machining: band saw −0 / +5 to +15 mm on length; waterjet +10 % of thickness on the diameter (min. 2 mm); machined parts −0 / +2 to +5 mm on the diameter. See the full tables (INF 002 and INF 003, the same for every alloy).
Tariff classification of Hastelloy C-22: NCM, HS, HTS and CN by product form
FormNCM (Brazil, 8 digits)HS (international, 6 digits)HTS (USA, 10 digits)*CN (European Union, 8 digits)*
Forged bar7505.12.107505.127505.12.30007505 12 00
Hot-rolled bar7505.12.107505.127505.12.30007505 12 00
Plate (> 10 mm, width ≥ 600 mm)7506.20.007506.207506.20.30007506 20 00
Seamless pipe7507.12.007507.127507.12.00007507 12 00
Welded pipe7507.12.007507.127507.12.00007507 12 00
Flange and fitting7507.20.007507.207507.20.00007507 20 00

Tariff class: nickel alloy (by chemical composition, under the Chapter 72 Notes and Section XV Note 5).

*: US and EU codes for reference. NCM per current legislation (General Rules of Interpretation, Notes to Chapters 72, 74 and 75 and Section XV Note 5). Confirm the final code with your customs broker according to the item size and finish. HS = first 6 digits of the NCM.

Chemical composition (%)

ASTM B574 / B564 (UNS N06022)

Chemical composition of Hastelloy C-22 – UNS N06022, per ASTM B574 / B564 (UNS N06022)
ElementRange (%)
Ni balance (≈ 56)
Cr 20.0 – 22.5
Mo 12.5 – 14.5
W 2.5 – 3.5
Fe 2.0 – 6.0
Co ≤ 2.5
Mn ≤ 0.50
V ≤ 0.35
Si ≤ 0.08
C ≤ 0.015
P ≤ 0.02
S ≤ 0.02

Calculate the PREN of Hastelloy C-22 in the PREN calculator →

Mechanical properties

solution annealed (ASTM B564 / B574)

Mechanical properties of Hastelloy C-22 – UNS N06022
PropertyValue
Yield strength (0.2%) ≥ 310 MPa
Tensile strength ≥ 690 MPa
Elongation ≥ 45%

Typical physical properties

Typical values at 20 °C
PropertyValue
Density 8.69 g/cm³
Melting range 1,357 – 1,399 °C
Modulus of elasticity 206 GPa
Thermal conductivity (20 °C) 10.1 W/m·K
Thermal expansion (20–100 °C) 12.4 µm/m·K

Calculate the weight of Hastelloy C-22 bar, plate or pipe →

Heat treatment, welding and machining

ItemUsual practice
Service temperature An alloy for aqueous corrosion, from cryogenic up to 677 °C (bolting up to 427 °C) in the ASME (II-D) allowable stress tables, but corrosive service should stay well below that. Avoid prolonged exposure to 600 – 1,000 °C (precipitation of μ and P phases).
Heat treatment Solution annealing at ≈ 1,120 °C with rapid cooling (water or forced air). Not age hardenable.
Welding Good weldability. Consumables: AWS A5.14 ERNiCrMo-10 and AWS A5.11 ENiCrMo-10, also used to weld C276, 625, super-austenitics and super duplex when over-alloyed weld metal is wanted.
Machining Difficult: work hardens; use carbide, low speed, constant feed and abundant coolant.

Plan an open-die forging in Hastelloy C-22: reduction, slenderness and how much material to send →Simulate the cutting plan of the ingot or bar →

Filler metal for welding

The wire composition is usually not identical to the material: each page explains why.

Typical applications

  • Chemical processes with mixed oxidizing and reducing media
  • Chlorination and wet chlorine handling
  • Flue gas desulfurization (FGD)
  • Pulp and paper bleaching
  • Pharmaceuticals and fine chemicals
  • Incineration and waste treatment
  • Welding consumable and overlay

Alternatives: C276 in strongly reducing media (hot HCl, H₂SO₄); alloys 59 / 686 / C-2000 in borderline cases; 625 in moderate media, at lower cost.

Compare alloys by corrosive medium, concentration and temperature →

Hastelloy C-22: complete guide

What Hastelloy C-22 is

Hastelloy C-22 belongs to the family of nickel alloys, in the nickel-chromium-molybdenum group. It is not "a steel alloy": nickel is about 56% of the composition and iron is between 2 and 6%. It was developed from C-276 with more chromium and less molybdenum, to extend resistance to oxidizing media without losing resistance to reducing ones, and with low carbon and silicon to keep the weld heat-affected zone as resistant as the base metal.

Chemical composition and role of the elements

Chromium (20 – 22.5%) protects in oxidizing media; molybdenum (12.5 – 14.5%) and tungsten (2.5 – 3.5%) protect in reducing media and against pitting and crevice corrosion; iron is limited to 6% and carbon to 0.015%. The equivalent PREN, Cr + 3.3 (Mo + 0.5 W), is around 65 to 70.

Mechanical properties

Solution annealed, ASTM B574 requires a minimum yield strength of 310 MPa, minimum tensile strength of 690 MPa and minimum elongation of 45%. The alloy is not hardenable by heat treatment; strength increases only by cold work.

Corrosion and limits of use

C-22 resists nitric acid, wet chlorine, ferric and cupric chlorides, hypochlorites, oxidizing acid mixtures with chlorides, seawater, brines and also dilute hydrochloric and sulfuric acid, which makes it the choice for processes where the medium alternates between oxidizing and reducing. In hot concentrated hydrochloric acid, alloy B-2 is superior.

Applications

Waste incinerators and gas scrubbers, desulfurization absorbers, chemical and pharmaceutical reactors and exchangers, pulp bleaching equipment, effluent treatment, valve and pump components in oxidizing chloride media and protective weld overlays.

Supply forms and Dustre services

Round bars and blocks forged in open die, cut to size on a band saw, with rough or finish machining, solution annealing or annealing in our own furnaces and hardness, tensile and impact testing. All material is supplied with a 3.1 inspection certificate and heat traceability.

Frequently asked questions

What is the chemical composition of Hastelloy C-22?

Per ASTM B574 / B564 (UNS N06022): Ni balance (≈ 56); Cr 20.0 – 22.5; Mo 12.5 – 14.5; W 2.5 – 3.5; Fe 2.0 – 6.0; Co ≤ 2.5.

Which standards cover Hastelloy C-22?

Bar: ASTM B574. Forging: ASTM B564; B462 (flanges and fittings). Plate: ASTM B575. Tube: ASTM B622 (seamless), B619/B626 (welded).

Up to what temperature can Hastelloy C-22 be used?

An alloy for aqueous corrosion, from cryogenic up to 677 °C (bolting up to 427 °C) in the ASME (II-D) allowable stress tables, but corrosive service should stay well below that. Avoid prolonged exposure to 600 – 1,000 °C (precipitation of μ and P phases).

Which materials can replace Hastelloy C-22?

C276 in strongly reducing media (hot HCl, H₂SO₄); alloys 59 / 686 / C-2000 in borderline cases; 625 in moderate media, at lower cost.

Where to buy Hastelloy C-22 in Brazil?

Dustre supplies Hastelloy C-22 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

Need Hastelloy C-22?Bars, forgings and parts with EN 10204 3.1 certificate.

Forms and stock of Hastelloy C-22

Dustre supplies Hastelloy C-22 as bar, plate, pipe and tube and forgings and flanges, cut to size, with forged and machined parts to drawing (shafts, discs, rings and blocks) and a 3.1 certificate.

Not in stock at the moment: supplied to order, with lead time in the quotation.

See the full ready-to-ship stock · Request a quote for Hastelloy C-22

Where to buy Hastelloy C-22 in Brazil?

Dustre supplies Hastelloy C-22 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

See also

HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp

We use your data only to answer this quote. Privacy. · WhatsApp +55 11 98649-0075 · Mon–Thu 07:00–17:00 · Fri 07:00–16:00 (Brasília time)