Zeron 100 / F55 super duplex stainless steel: standards, composition and properties

UNS S32760, 1.4501

Download data sheet (PDF)

F55 is the ASTM A182 forging of super duplex UNS S32760, known by the trade name Zeron 100: austenitic-ferritic stainless with 24–26 % Cr, 3–4 % Mo, 0.20–0.30 % N and additions of copper and tungsten (0.5–1.0 % each), with PREN ≥ 40 required by purchase specifications (NORSOK M-630, manufacturer) and a yield strength of 550 MPa. In EN it is 1.4501; as a casting, grade 6A (CD3MWCuN). F53 (S32750, 2507) is another super duplex, without Cu and W, and has its own page.

Technical review Oct 2026 · * value to be confirmed in the current edition of the standard

UNSS32760 (Zeron 100); equivalent casting J93380 (6A)
EN / W.Nr.1.4501 X2CrNiMoCuWN25-7-4
PREN≥ 40 required by ASTM itself (Cr + 3.3(Mo + 0.5 W) + 16 N)
YS / UTS min.550 / 750–895 MPa (F55 forging)
Ferrite35–55 % is the usual purchase range (NORSOK); ASTM does not fix it

One composition, several standards

The name changes with the product form. When specifying, cite the standard, grade and class.

Standards for Super duplex Zeron 100 / F55 / S32760 by product form
FormASTM/ASMEGrade/classENABNT/others
Forging and flange (B16.5) A182 / SA-182F55 (S32760)EN 10250-4 / EN 10222-5: 1.4501*NORSOK M-630 MDS D54
Bar A479 / SA-479; A276S32760EN 10088-3 / EN 10272: 1.4501NORSOK MDS D57
Plate, coil, strip A240 / SA-240S32760EN 10088-2 / EN 10028-7: 1.4501NORSOK MDS D55
Seamless pipe (line) A790 / SA-790S32760EN 10216-5: 1.4501NORSOK MDS D51
Heat exchanger tube A789 / SA-789S32760EN 10216-5NORSOK MDS D58
Welded pipe A790 (welded); A928 (fusion welded, classes 1–5)S32760EN 10217-7: 1.4501NORSOK MDS D52
Fittings (butt-weld) A815 / SA-815WPS32760 (classes WP-S, WP-W, WP-WX, CR)*EN 10253-4NORSOK MDS D53
Casting A890 / A995 (pressure)6A = CD3MWCuN (J93380)—NORSOK MDS D56
Welding consumable AWS A5.9 / A5.4 / A5.22ER2594, E2594, E2594T; Zeron 100X typeEN ISO 14343: 25 9 4 N LZeron 100X (with W) matches S32760
Washer/bolt, sour service A182 / A479 / A276 + NACES32760—NACE MR0175/ISO 15156-3; NACE MR0103; API 6A*

NBR 5601 has no super duplex grade; specify by UNS + ASTM/EN product standard.

Tolerances and HS codes

  • Forged bars (round and square): machining allowance from 2 mm (Ø 6–16 mm) to 24 mm (Ø 400–500 mm) on the diameter. E.g. Ø 100–125 mm finished: +7 mm, tolerance +6 / −0 (length up to 3,500 mm).
  • Forged discs: allowance of 4 to 9 mm on the diameter and 3 to 11 mm on the height, plus-only tolerance.
  • Cutting and machining: band saw −0 / +5 to +15 mm on length; waterjet +10 % of thickness on the diameter (min. 2 mm); machined parts −0 / +2 to +5 mm on the diameter. See the full tables (INF 002 and INF 003, the same for every alloy).
Tariff classification of Super duplex Zeron 100 / F55 / S32760: NCM, HS, HTS and CN by product form
FormNCM (Brazil, 8 digits)HS (international, 6 digits)HTS (USA, 10 digits)*CN (European Union, 8 digits)*
Forged bar7222.30.007222.307222.30.00247222 30 51
Hot-rolled bar7222.11.007222.117222.11.00597222 11 11
Plate (> 10 mm, width ≥ 600 mm)7219.21.007219.217219.21.00207219 21 10
Seamless pipe7304.41.907304.417304.41.60457304 41 00
Welded pipe7306.40.007306.407306.40.50857306 40 80
Flange and fitting7307.21.007307.217307.21.50007307 21 00

Tariff class: stainless steel (by chemical composition, under the Chapter 72 Notes and Section XV Note 5).

*: US and EU codes for reference. NCM per current legislation (General Rules of Interpretation, Notes to Chapters 72, 74 and 75 and Section XV Note 5). Confirm the final code with your customs broker according to the item size and finish. HS = first 6 digits of the NCM.

Chemical composition by standard (%)

The ranges of each standard side by side, to see where they differ.

Chemical composition of Super duplex Zeron 100 / F55 / S32760 by standard, in %
Standard / gradeC maxMn maxP maxS maxSi maxCrNiMoNOthers
A240/A182 F55 (S32760) 0.0301.000.0300.0101.0024.0–26.06.0–8.03.0–4.00.20–0.30Cu 0.50–1.00; W 0.50–1.00; PREN ≥ 40
A890/A995 6A (CD3MWCuN) 0.031.000.0300.0251.0024.0–26.06.5–8.53.0–4.00.20–0.30Cu 0.5–1.0; W 0.5–1.0

Calculate the PREN of Super duplex Zeron 100 / F55 / S32760 in the PREN calculator →

Mechanical properties by standard

Minimum values at room temperature, in the stated delivery condition.

Minimum mechanical properties of Super duplex Zeron 100 / F55 / S32760
Standard and conditionYS minUTSElong.RAHardness
FORGINGS
A182 F55, solution annealed 550 MPa (80 ksi)750–895 MPa (109–130 ksi)25 %45 %not specified by A182
ROLLED
A240 S32760, plate 550 MPa750–895 MPa25 %——
PIPE, FITTINGS AND CASTINGS
A790 / A789 S32760 550 MPa≥ 750 MPa25 %—310 HBW / 32 HRC max
A890 / A995 6A (CD3MWCuN) 450 MPa (65 ksi)690 MPa min (100 ksi)25 %——

Calculate the weight of Super duplex Zeron 100 / F55 / S32760 bar, plate or pipe →

F55 (S32760) vs. F53 (S32750): Zeron 100 vs. 2507

Both alloys share the same 25Cr-7Ni base and the same 550 MPa YS. S32750 (2507) uses more Mo (up to 5 %) and N (0.24–0.32 %) and has no W; it has a higher minimum UTS (800 MPa) and lower elongation (15 %). S32760 (Zeron 100) adds Cu and W (0.5–1.0 % each), has Mo max 4 % and carries PREN ≥ 40 as a requirement in the composition itself; UTS sits at 750–895 MPa with 25 % elongation. In practice they are interchangeable in many MDS (NORSOK lists both on the same data sheet), but they are not the same grade: check which UNS the specification requires, and use a compatible consumable (ER2594 or Zeron 100X type).

Heat treatments required by the standards

Delivery conditions and temperatures
StandardDelivery conditionTemperature
A182 F55 / A240 S32760 Solution annealed and liquid cooled1100–1140 °C (2010–2085 °F)
A790 S32760 Solution annealed and rapidly cooled1070–1140 °C (1960–2085 °F)
A890 / A995 6A Solution annealed and water quenched1100 °C min*

Plan an open-die forging in Super duplex Zeron 100 / F55 / S32760: reduction, slenderness and how much material to send →Simulate the cutting plan of the ingot or bar →

Variants in the family

Variants of Super duplex Zeron 100 / F55 / S32760
VariantStandardsDifferenceYS / UTS
S32750 (2507, SAF 2507, 1.4410) A182 F53, A240, A479, A790, A789, A815, A928Mo 3–5 %, N 0.24–0.32 %, no W/Cu550 / 800 MPa
S32760 (Zeron 100, 1.4501) A182 F55, A240, A276, A479, A790, A789, A815, A928Cu 0.5–1 % and W 0.5–1 %; PREN ≥ 40 required550 / 750–895 MPa
S32550 (Ferralium 255, 1.4507) A182 F61, A240, A479, A276, A790Cu 1.5–2.5 %, lower Ni and N; minimum PREN may be < 40550 / 750–760 MPa
S32520 (UR 52N+, Ferralium 255-SD50, 1.4507) A182 F59, A240, A789, A790, A928Cu 0.5–3 %*, N up to 0.35 %; PREN > 40550 / 770 MPa
CE3MN (5A, J93404) A890 / A995 5ACasting equivalent to 2507; Mo 4–5 %515 / 690 MPa
CD3MWCuN (6A, J93380) A890 / A995 6ACasting equivalent to Zeron 100 (Cu + W)450 / 690 MPa

Corrosion, PREN and temperature

  • PREN: Cr + 3.3 (Mo + 0.5 W) + 16 N. For S32760, NORSOK M-630, NACE MR0175 and the manufacturer specification (Zeron 100) require PREN ≥ 40; with the ASTM minimum contents the calculation gives ≈ 38, which is why the PREN is checked on the heat.
  • Pitting and crevice corrosion: the usual test is ASTM G48 method A at 50 °C for 24 h, no pitting (22Cr: 40 °C). Typical CPT well above that of 22Cr duplex and 316L.
  • Intermetallic phases (sigma, chi): precipitate quickly between ~600 and 1000 °C; the critical formation range goes from ~320 to 955 °C (A923). Slow cooling after solution annealing or welding with high heat input collapses toughness and pitting resistance.
  • 475 °C embrittlement: the ferrite hardens with long exposure between ~300 and 525 °C, which limits continuous use to about 250 °C (ASME usually accepts up to ~315 °C)*.
  • Low temperature: toughness proven by Charpy at −46 °C (NORSOK: 45 J average / 35 J individual) or −40 °C (A923 method B).
  • NACE MR0175/ISO 15156-3: solution-annealed super duplex is accepted with pH2S, chloride and temperature limits that depend on the PREN range (40–45); NACE MR0103 limits super duplex to 32 HRC; NORSOK purchases usually require 28 HRC / 270 HB*.

Compare alloys by corrosive medium, concentration and temperature →

Tests required for super duplex (ASTM A923, G48, NORSOK)

  • ASTM A923: detects intermetallic phases: method A (NaOH etch, acceptance only), method B (Charpy) and method C (ferric chloride).
  • A923 method C: S32750, S32550 and S32520 tested at 40 °C, maximum loss 10 mdd.
  • A923 method B: S32750 at −40 °C with energy agreed between purchaser and supplier; casting J93404 (5A) at −46 °C, 54 J min.
  • ASTM G48 A at 50 °C / 24 h: no pitting and mass loss ≤ 4 g/m² is the usual NORSOK M-630/M-650 criterion*.
  • Ferrite (ASTM E562): 35–55 % in the base metal (typical); in the weld, the range required by NORSOK M-601.
  • NORSOK M-650: manufacturer qualification (forge, foundry, mill) for 25Cr; requires a qualification piece with the tests above.

Welding

Usual welding practice
ItemUsual practice
Consumable ER2594 (AWS A5.9), E2594 (A5.4) or a Zeron 100X type consumable (with W); EN ISO 14343 25 9 4 N L
Gas Ar + 2 % N2 (shielding) and Ar or Ar + N2 for purging, to avoid nitrogen loss at the root
Preheat Not used
Interpass Max 100–150 °C (100 °C common for 25Cr)*
Heat input Low and controlled, ~0.5–1.5 kJ/mm, to balance ferrite without precipitating sigma*
PWHT No stress relief is done; if needed, only full solution annealing with water quenching
Control Ferrite and hardness in qualification (350 HV10 max usual), G48 and Charpy per NORSOK M-601/M-650*

Filler metal for welding

The wire composition is usually not identical to the material: each page explains why.

International equivalents

Equivalent designations
SystemDesignation
UNS S32760; equivalent casting J93380 (6A)
ASTM forging F55 (S32760)
EN / W.Nr. 1.4501 X2CrNiMoCuWN25-7-4
Trade names Zeron 100 (Rolled Alloys)
JIS No direct JIS equivalent
GB 022Cr25Ni7Mo4WCuN (S27603), GB/T 20878
ABNT / SAE / AISI No AISI/SAE designation; NBR 5601 has no corresponding grade*

Equivalence is by approximate composition; minimum properties, tests and heat treatment change from standard to standard.

Typical applications

Form or industryWhere it is used
Offshore oil and gas Seawater lines, injection, manifolds, umbilicals and firewater systems (NORSOK)
Subsea Connectors, F55 flanges, hubs and valves in contact with seawater
Desalination (SWRO) High-pressure pipes and vessels with brine
Chemicals and pulp Exchangers, pumps and equipment with chlorides and acids
Pumps and valves Cast 6A bodies, shafts and internals in A479 bar
Fastening Super duplex studs and nuts for chloride and H2S service

Frequently asked questions

Are F53 and F55 the same thing?

No. F53 is S32750 (2507) and F55 is S32760 (Zeron 100, with Cu and W). They have the same 550 MPa YS and 25Cr base, but composition, UTS and heat treatment differ.

What is the minimum PREN of F55?

PREN ≥ 40, required by purchase specifications (NORSOK M-630, NACE MR0175 and the manufacturer) and checked on the heat analysis: Cr + 3.3 (Mo + 0.5 W) + 16 N. With the ASTM minimum contents alone the calculation would give ≈ 38.

What is the difference between duplex and super duplex?

22Cr duplex (S31803/S32205, F51/F60) has PREN ~34 and YS 450 MPa. 25Cr super duplex has PREN ≥ 40 and YS 550 MPa, for seawater and more aggressive chlorides.

Which casting corresponds to Zeron 100?

ASTM A890/A995 grade 6A (CD3MWCuN, J93380), with Cu and W like S32760.

Need Super duplex Zeron 100 / F55 / S32760?Bars, forgings and parts with EN 10204 3.1 certificate.

Forms and stock of Super duplex Zeron 100 / F55 / S32760

Dustre supplies Super duplex Zeron 100 / F55 / S32760 as bar, plate, pipe and tube, forgings and flanges, fittings and castings, cut to size, with forged and machined parts to drawing (shafts, discs, rings and blocks) and a 3.1 certificate.

In stock in Osasco/SP, Brazil: round bar from Ø 2 to 406 mm. List updated on 11/13/2026.

See the full ready-to-ship stock · Request a quote for Super duplex Zeron 100 / F55 / S32760

Where to buy Super duplex Zeron 100 / F55 / S32760 in Brazil?

Dustre supplies Super duplex Zeron 100 / F55 / S32760 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

See also

HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp

We use your data only to answer this quote. Privacy. · WhatsApp +55 11 98649-0075 · Mon–Thu 07:00–17:00 · Fri 07:00–16:00 (Brasília time)