316Ti stainless steel – UNS S31635

Titanium-stabilized Cr-Ni-Mo austenitic stainless steel

Download data sheet (PDF)

Variant of 316 with titanium (≥ 5×(C+N)), which ties up carbon as Ti carbide and prevents sensitization in welding and in service between 425 and 815 °C. Corrosion resistance equivalent to 316; preferred in thick sections and hot service.

Technical review Oct 2026 · minimum values per the cited standard; physical properties are typical; values marked * to be confirmed in the standard

FamilyAustenitic stainless
UNSS31635
W.Nr. / EN1.4571 (X6CrNiMoTi17-12-2)
PREN≈ 23 – 28 (typical ≈ 25)

Designations and equivalents

Designations of 316Ti stainless steel – UNS S31635
SystemDesignation
UNS S31635
W.Nr./EN 1.4571 (X6CrNiMoTi17-12-2)
DIN X6CrNiMoTi17-12-2
JIS SUS316Ti
Trade names AISI 316Ti
Others V4A (DE)

Standards by product form

Standards for 316Ti stainless steel – UNS S31635
FormStandard
Bar ASTM A479 / EN 10088-3
Forging/flange ASTM A182 F316Ti
Plate ASTM A240
Tube ASTM A312 TP316Ti

Tolerances and HS codes

  • Forged bars (round and square): machining allowance from 2 mm (Ø 6–16 mm) to 24 mm (Ø 400–500 mm) on the diameter. E.g. Ø 100–125 mm finished: +7 mm, tolerance +6 / −0 (length up to 3,500 mm).
  • Forged discs: allowance of 4 to 9 mm on the diameter and 3 to 11 mm on the height, plus-only tolerance.
  • Cutting and machining: band saw −0 / +5 to +15 mm on length; waterjet +10 % of thickness on the diameter (min. 2 mm); machined parts −0 / +2 to +5 mm on the diameter. See the full tables (INF 002 and INF 003, the same for every alloy).
Tariff classification of 316Ti stainless steel: NCM, HS, HTS and CN by product form
FormNCM (Brazil, 8 digits)HS (international, 6 digits)HTS (USA, 10 digits)*CN (European Union, 8 digits)*
Forged bar7222.30.007222.307222.30.00247222 30 51
Hot-rolled bar7222.11.007222.117222.11.00597222 11 11
Plate (> 10 mm, width ≥ 600 mm)7219.21.007219.217219.21.00207219 21 10
Seamless pipe7304.41.907304.417304.41.60457304 41 00
Welded pipe7306.40.007306.407306.40.50857306 40 80
Flange and fitting7307.21.007307.217307.21.50007307 21 00

Tariff class: stainless steel (by chemical composition, under the Chapter 72 Notes and Section XV Note 5).

*: US and EU codes for reference. NCM per current legislation (General Rules of Interpretation, Notes to Chapters 72, 74 and 75 and Section XV Note 5). Confirm the final code with your customs broker according to the item size and finish. HS = first 6 digits of the NCM.

Chemical composition (%)

ASTM A182 F316Ti / A479

Chemical composition of 316Ti stainless steel – UNS S31635, per ASTM A182 F316Ti / A479
ElementRange (%)
C ≤ 0.08
Mn ≤ 2.00
P ≤ 0.045
S ≤ 0.030
Si ≤ 1.00
Cr 16.0 – 18.0
Ni 10.0 – 14.0
Mo 2.00 – 3.00
N ≤ 0.10
Ti 5×(C+N) – 0.70
Fe balance

Calculate the PREN of 316Ti stainless steel in the PREN calculator →

Mechanical properties

Solution annealed (ASTM A182 F316Ti)

Mechanical properties of 316Ti stainless steel – UNS S31635
PropertyValue
Yield strength (0.2%) ≥ 205 MPa
Tensile strength ≥ 515 MPa
Elongation ≥ 30%
Reduction of area ≥ 40%
Hardness ≤ 217 HB (typical)

Typical physical properties

Typical values at 20 °C
PropertyValue
Density 8.0 g/cm³
Melting range 1,375 – 1,400 °C
Modulus of elasticity 200 GPa
Thermal conductivity (20 °C) ≈ 15 W/m·K
Thermal expansion (20–100 °C) ≈ 16.5 µm/m·K

Calculate the weight of 316Ti stainless steel bar, plate or pipe →

Heat treatment, welding and machining

ItemUsual practice
Service temperature Cryogenic up to ≈ 800 °C (stabilized against sensitization); oxidation ≈ 870 °C.
Heat treatment Solution annealing 1,020 – 1,120 °C with rapid cooling. Optional stabilizing anneal ≈ 870–900 °C.
Welding Good. Ti does not transfer well across the arc: use ER318 (Nb-stabilized 316) or ER316L; E318/E316L for covered electrode.
Machining Machinability lower than carbon steel: it work hardens quickly; use sharp tools, positive rake, constant feed without 'rubbing' and abundant coolant. Ti carbonitrides increase tool wear.

Plan an open-die forging in 316Ti stainless steel: reduction, slenderness and how much material to send →Simulate the cutting plan of the ingot or bar →

Filler metal for welding

The wire composition is usually not identical to the material: each page explains why.

Typical applications

  • Chemical equipment in thick sections
  • Exchangers and vessels operating between 400 and 800 °C
  • Exhaust manifolds and expansion joints
  • Pulp and paper
  • Welded parts that cannot be solution annealed

Alternatives: 316L is enough for service up to ≈ 425 °C (more available); 316H for creep resistance; 317L/904L for more severe corrosion.

Compare alloys by corrosive medium, concentration and temperature →

316Ti stainless steel: complete guide

What 316Ti stainless steel is

316Ti belongs to the family of austenitic stainless steels. It has the same base as 316L, 16 – 18% chromium, 10 – 14% nickel and 2 – 3% molybdenum, but solves sensitization differently: instead of limiting carbon, it adds titanium in an amount of at least five times the sum of carbon and nitrogen. Titanium forms stable carbides and leaves the chromium free to form the passive film.

Chemical composition and role of the elements

Molybdenum mainly increases resistance to pitting and crevice corrosion in chlorides. Titanium stabilizes the steel against chromium carbide precipitation in long exposures at 450 – 800 °C, a situation in which 316L can also sensitize over time. Nitrogen is limited to 0.10% because it consumes titanium.

Welding and magnetism

Weldable by all processes, without preheating or post-weld heat treatment, with ER318 or ER316L consumables. In the solution-annealed condition it is practically non-magnetic; slight magnetism appears only after cold work, from the formation of strain-induced martensite.

Service temperature and corrosion

Corrosion resistance is that of 316L, with PREN ≈ 23 – 28; in stagnant or heated seawater it suffers pitting and crevice corrosion.

Applications

Heat exchangers, reactors and process piping that operate hot, pulp and paper equipment, exhaust and components exposed to thermal cycling, shafts and machined parts replacing 316L when there is service at temperature.

Supply forms and Dustre services

Round bars and blocks forged in open die, cut to size on a band saw, with rough or finish machining, solution annealing in our own furnaces and hardness, tensile and impact testing. All material is supplied with a 3.1 inspection certificate and heat traceability.

Frequently asked questions

What is the chemical composition of 316Ti stainless steel?

Per ASTM A182 F316Ti / A479: C ≤ 0.08; Mn ≤ 2.00; P ≤ 0.045; S ≤ 0.030; Si ≤ 1.00; Cr 16.0 – 18.0.

Which standards cover 316Ti stainless steel?

Bar: ASTM A479 / EN 10088-3. Forging/flange: ASTM A182 F316Ti. Plate: ASTM A240. Tube: ASTM A312 TP316Ti.

Up to what temperature can 316Ti stainless steel be used?

Cryogenic up to ≈ 800 °C (stabilized against sensitization); oxidation ≈ 870 °C.

Which materials can replace 316Ti stainless steel?

316L is enough for service up to ≈ 425 °C (more available); 316H for creep resistance; 317L/904L for more severe corrosion.

Where to buy 316Ti stainless steel in Brazil?

Dustre supplies 316Ti stainless steel as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

Need 316Ti stainless steel?Bars, forgings and parts with EN 10204 3.1 certificate.

Forms and stock of 316Ti stainless steel

Dustre supplies 316Ti stainless steel as bar, plate, pipe and tube and forgings and flanges, cut to size, with forged and machined parts to drawing (shafts, discs, rings and blocks) and a 3.1 certificate.

In stock in Osasco/SP, Brazil: round bar from Ø 25.4 to 101.6 mm. List updated on 11/13/2026.

See the full ready-to-ship stock · Request a quote for 316Ti stainless steel

Where to buy 316Ti stainless steel in Brazil?

Dustre supplies 316Ti stainless steel as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

See also

HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp