Inconel 718 – UNS N07718

Precipitation-hardenable nickel-chromium superalloy

Download data sheet (PDF)

Ni-Cr-Fe superalloy hardened by precipitation of γ″ (Ni₃Nb). It reaches a yield strength above 1,000 MPa and keeps its strength up to ~650 °C. The slow precipitation allows welding without strain-age cracking. It is the most used high-strength alloy in aircraft turbines and in wellhead equipment (API Std 6ACRA, which replaced the former 6A718).

Technical review Oct 2026 · minimum values per the cited standard; physical properties are typical; values marked * to be confirmed in the standard

FamilyNickel alloy
UNSN07718
W.Nr. / EN2.4668 – NiCr19Fe19Nb5Mo3

Designations and equivalents

Designations of Inconel 718 – UNS N07718
SystemDesignation
UNS N07718
W.Nr./EN 2.4668 – NiCr19Fe19Nb5Mo3
DIN NiCr19NbMo
JIS NCF 718
Trade names Inconel 718 (Special Metals), Haynes 718, ATI 718, Alloy 718
Others AMS 5662 / 5663 / 5664 (bar and forging), AMS 5596 (sheet), API 6ACRA

Standards by product form

Standards for Inconel 718 – UNS N07718
FormStandard
Bar ASTM B637; AMS 5662 / 5663
Forging ASTM B637; AMS 5663; API 6ACRA (oil and gas)
Plate ASTM B670; AMS 5596 / 5597
Tube AMS 5589 / 5590

Tolerances and HS codes

  • Forged bars (round and square): machining allowance from 2 mm (Ø 6–16 mm) to 24 mm (Ø 400–500 mm) on the diameter. E.g. Ø 100–125 mm finished: +7 mm, tolerance +6 / −0 (length up to 3,500 mm).
  • Forged discs: allowance of 4 to 9 mm on the diameter and 3 to 11 mm on the height, plus-only tolerance.
  • Cutting and machining: band saw −0 / +5 to +15 mm on length; waterjet +10 % of thickness on the diameter (min. 2 mm); machined parts −0 / +2 to +5 mm on the diameter. See the full tables (INF 002 and INF 003, the same for every alloy).
Tariff classification of Inconel 718: NCM, HS, HTS and CN by product form
FormNCM (Brazil, 8 digits)HS (international, 6 digits)HTS (USA, 10 digits)*CN (European Union, 8 digits)*
Forged bar7505.12.107505.127505.12.30007505 12 00
Hot-rolled bar7505.12.107505.127505.12.30007505 12 00
Plate (> 10 mm, width ≥ 600 mm)7506.20.007506.207506.20.30007506 20 00
Seamless pipe7507.12.007507.127507.12.00007507 12 00
Welded pipe7507.12.007507.127507.12.00007507 12 00
Flange and fitting7507.20.007507.207507.20.00007507 20 00

Tariff class: nickel alloy (by chemical composition, under the Chapter 72 Notes and Section XV Note 5).

*: US and EU codes for reference. NCM per current legislation (General Rules of Interpretation, Notes to Chapters 72, 74 and 75 and Section XV Note 5). Confirm the final code with your customs broker according to the item size and finish. HS = first 6 digits of the NCM.

Chemical composition (%)

ASTM B637 / AMS 5662 (UNS N07718)

Chemical composition of Inconel 718 – UNS N07718, per ASTM B637 / AMS 5662 (UNS N07718)
ElementRange (%)
Ni (+Co) 50.0 – 55.0
Cr 17.0 – 21.0
Fe balance (≈ 18)
Nb + Ta 4.75 – 5.50
Mo 2.80 – 3.30
Ti 0.65 – 1.15
Al 0.20 – 0.80
Co ≤ 1.00
C ≤ 0.08
Mn ≤ 0.35
Si ≤ 0.35
Cu ≤ 0.30
B ≤ 0.006
P / S ≤ 0.015 / ≤ 0.015

Calculate the PREN of Inconel 718 in the PREN calculator →

Mechanical properties

solution treated + aged (AMS 5663 / ASTM B637)

Mechanical properties of Inconel 718 – UNS N07718
PropertyValue
Yield strength (0.2%) ≥ 1,034 MPa
Tensile strength ≥ 1,276 MPa
Elongation ≥ 12%
Reduction of area ≥ 15%
Hardness ≥ 331 HB
API 6ACRA (oil and gas) YS 827 – 1,000 MPa; UTS ≥ 1,034 MPa; El. ≥ 20%; RA ≥ 35%; 32 – 40 HRC; Charpy ≥ 47 J at −60 °C

Typical physical properties

Typical values at 20 °C
PropertyValue
Density 8.19 g/cm³
Melting range 1,260 – 1,336 °C
Modulus of elasticity 200 GPa
Thermal conductivity (20 °C) 11.4 W/m·K
Thermal expansion (20–100 °C) 13.0 µm/m·K
Electrical resistivity 125 µΩ·cm

Calculate the weight of Inconel 718 bar, plate or pipe →

Heat treatment, welding and machining

ItemUsual practice
Service temperature From cryogenic (−253 °C) up to ~650 °C with structural strength; above that the γ″ phase coarsens and strength drops. Oxidation acceptable up to ~980 °C.
Heat treatment AMS 5663: solution treat at 940 – 1,010 °C (typically 980 °C) and cool rapidly; age at 720 °C for 8 h, furnace cool at ~55 °C/h to 620 °C and hold until 18 h total, air cooling. API 6ACRA: solution treat at 1,021 – 1,052 °C and age at 774 – 802 °C for 6 – 8 h.
Welding Good weldability for a hardenable alloy (low tendency to strain-age cracking). Consumable AWS A5.14 ERNiFeCr-2. Weld in the solution-treated condition and age afterwards.
Machining Very difficult, especially aged: rough machine in the solution-treated condition; use carbide or ceramic, low speed and a rigid tool.

Plan an open-die forging in Inconel 718: reduction, slenderness and how much material to send →Simulate the cutting plan of the ingot or bar →

Filler metal for welding

The wire composition is usually not identical to the material: each page explains why.

Typical applications

  • Discs, shafts and casings of aircraft gas turbines
  • Wellhead and completion equipment (API 6A, NACE MR0175)
  • Hangers, mandrels and downhole valves
  • High-strength fasteners and springs
  • Rocket engines and cryogenic components
  • Hot-work tooling

Alternatives: Inconel 625 when corrosion and weldability weigh more than strength; 725 in oil and gas with more severe H₂S; Waspaloy or 718Plus above 650 °C; Monel K500 for seawater with lower strength and cost.

Compare alloys by corrosive medium, concentration and temperature →

Inconel 718: complete guide

What Inconel 718 is

Inconel 718 belongs to the family of nickel alloys, in the group of precipitation-hardenable superalloys. It is not "a special steel alloy": nickel is more than half of the composition and iron, about 18%, is just one of the alloying elements. Strength comes from two precipitates formed during aging, gamma double prime (Ni3Nb), produced by niobium, and gamma prime (Ni3(Al,Ti)); the slow kinetics of the former is what makes 718 the easiest superalloy to weld and fabricate.

Chemical composition

The ASTM B637 limits are: nickel from 50 to 55%, chromium from 17 to 21%, niobium plus tantalum from 4.75 to 5.50%, molybdenum from 2.80 to 3.30%, titanium from 0.65 to 1.15%, aluminum from 0.20 to 0.80%, carbon up to 0.08% and iron as the balance.

Mechanical properties by specification

Solution treated and aged per AMS 5663, the alloy has a minimum yield strength of 1,034 MPa, minimum tensile strength of 1,276 MPa, minimum elongation of 12% and minimum hardness of 331 HBW. In the wellhead equipment version, API 6ACRA, the yield strength is between 827 and 1,000 MPa, the minimum tensile strength is 1,034 MPa, the minimum elongation 20% and the maximum hardness 40 HRC, to meet NACE MR0175.

Corrosion, temperature and applications

718 resists seawater, chlorides, H2S and CO2, organic acids and moderately oxidizing media, similarly to Inconel 625, and keeps its mechanical strength from −253 °C up to about 650 °C. It is used in discs, shafts, casings and fasteners of aircraft and gas turbines, in christmas trees, valves and connectors of oil wells, in high-strength bolts and studs and in cryogenic components. For fasteners up to 700 °C at lower cost, A-286 is the alternative.

Supply forms and Dustre services

Round bars and blocks forged in open die, cut to size on a band saw, with rough or finish machining, solution annealing or annealing in our own furnaces and hardness, tensile and impact testing. All material is supplied with a 3.1 inspection certificate and heat traceability.

Frequently asked questions

What is the chemical composition of Inconel 718?

Per ASTM B637 / AMS 5662 (UNS N07718): Ni (+Co) 50.0 – 55.0; Cr 17.0 – 21.0; Fe balance (≈ 18); Nb + Ta 4.75 – 5.50; Mo 2.80 – 3.30; Ti 0.65 – 1.15.

Which standards cover Inconel 718?

Bar: ASTM B637; AMS 5662 / 5663. Forging: ASTM B637; AMS 5663; API 6ACRA (oil and gas). Plate: ASTM B670; AMS 5596 / 5597. Tube: AMS 5589 / 5590.

Up to what temperature can Inconel 718 be used?

From cryogenic (−253 °C) up to ~650 °C with structural strength; above that the γ″ phase coarsens and strength drops. Oxidation acceptable up to ~980 °C.

Which materials can replace Inconel 718?

Inconel 625 when corrosion and weldability weigh more than strength; 725 in oil and gas with more severe H₂S; Waspaloy or 718Plus above 650 °C; Monel K500 for seawater with lower strength and cost.

Where to buy Inconel 718 in Brazil?

Dustre supplies Inconel 718 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

Need Inconel 718?Bars, forgings and parts with EN 10204 3.1 certificate.

Forms and stock of Inconel 718

Dustre supplies Inconel 718 as bar, plate, pipe and tube and forgings and flanges, cut to size, with forged and machined parts to drawing (shafts, discs, rings and blocks) and a 3.1 certificate.

In stock in Osasco/SP, Brazil: round bar from Ø 12.7 to 203 mm. List updated on 11/13/2026.

See the full ready-to-ship stock · Request a quote for Inconel 718

Where to buy Inconel 718 in Brazil?

Dustre supplies Inconel 718 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

See also

HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp

We use your data only to answer this quote. Privacy. · WhatsApp +55 11 98649-0075 · Mon–Thu 07:00–17:00 · Fri 07:00–16:00 (Brasília time)