ASTM A182 F9 – UNS K90941

Forged 9Cr-1Mo steel for high temperature and sulfidizing media

Download data sheet (PDF)

Cr-Mo steel with 8–10% Cr and 1% Mo, forged to ASTM A182. It has oxidation and sulfidation resistance superior to F5 and is used in furnaces and hot refinery lines. For high pressure/creep, the modified grade F91 (with V, Nb, N) has replaced it in many applications.

Technical review Oct 2026 · minimum values per the cited standard; physical properties are typical; values marked * to be confirmed in the standard

FamilyAlloy steel
UNSK90941
W.Nr. / ENX11CrMo9-1 – 1.7386 (EN 10216-2 / 10222-2)

Designations and equivalents

Designations of ASTM A182 F9 – UNS K90941
SystemDesignation
UNS K90941
W.Nr./EN X11CrMo9-1 – 1.7386 (EN 10216-2 / 10222-2)
DIN X12CrMo9-1 (X12CrMo91, old)
JIS SFVAF9 (JIS G3203)
Trade names 9Cr-1Mo, F9
Others Pipe A335 P9; plate A387 Gr 9; fittings A234 WP9; casting A217 C12

Standards by product form

Standards for ASTM A182 F9 – UNS K90941
FormStandard
Forging (flanges, fittings, valves) ASTM A182/A182M F9; ASME SA-182
Larger forgings ASTM A336 F9
Pipe/tube ASTM A335 P9 / A213 T9
Plate ASTM A387 Gr 9
Butt-welding fittings ASTM A234 WP9
Casting ASTM A217 C12

Tolerances and HS codes

  • Forged bars (round and square): machining allowance from 2 mm (Ø 6–16 mm) to 24 mm (Ø 400–500 mm) on the diameter. E.g. Ø 100–125 mm finished: +7 mm, tolerance +6 / −0 (length up to 3,500 mm).
  • Forged discs: allowance of 4 to 9 mm on the diameter and 3 to 11 mm on the height, plus-only tolerance.
  • Cutting and machining: band saw −0 / +5 to +15 mm on length; waterjet +10 % of thickness on the diameter (min. 2 mm); machined parts −0 / +2 to +5 mm on the diameter. See the full tables (INF 002 and INF 003, the same for every alloy).
Tariff classification of ASTM A182 F9: NCM, HS, HTS and CN by product form
FormNCM (Brazil, 8 digits)HS (international, 6 digits)HTS (USA, 10 digits)*CN (European Union, 8 digits)*
Forged bar7228.40.007228.407228.40.00007228 40 90
Plate (> 10 mm, width ≥ 600 mm)7225.40.907225.407225.40.30507225 40 40
Seamless pipe7304.19.007304.197304.19.50507304 19 10
Welded pipe7306.19.007306.197306.19.51507306 19 00
Flange and fitting7307.91.007307.917307.91.50307307 91 00

Tariff class: alloy steel (by chemical composition, under the Chapter 72 Notes and Section XV Note 5).

Pipe: 7304.19 and 7306.19 are line pipe for oil and gas pipelines; boiler, heat exchanger or process tubes go under 7304.39/7304.59 (seamless) and 7306.30/7306.50 (welded).

*: US and EU codes for reference. NCM per current legislation (General Rules of Interpretation, Notes to Chapters 72, 74 and 75 and Section XV Note 5). Confirm the final code with your customs broker according to the item size and finish. HS = first 6 digits of the NCM.

Chemical composition (%)

ASTM A182/A182M – F9

Chemical composition of ASTM A182 F9 – UNS K90941, per ASTM A182/A182M – F9
ElementRange (%)
C ≤ 0.15
Mn 0.30 – 0.60
P ≤ 0.030
S ≤ 0.030
Si 0.50 – 1.00
Cr 8.0 – 10.0
Mo 0.90 – 1.10

Calculate the carbon equivalent of ASTM A182 F9 for welding →

Mechanical properties

Annealed or normalized + tempered – ASTM A182 F9

Mechanical properties of ASTM A182 F9 – UNS K90941
PropertyValue
Yield strength (0.2%) ≥ 380 MPa
Tensile strength ≥ 585 MPa
Elongation ≥ 20%
Reduction of area ≥ 40%
Hardness 179 – 217 HBW

Typical physical properties

Typical values at 20 °C
PropertyValue
Density 7.75 g/cm³ (typical)
Modulus of elasticity ≈ 210 GPa (typical)
Thermal conductivity (20 °C) ≈ 27 W/m·K (typical)
Thermal expansion (20–100 °C) ≈ 10.9 µm/m·K (typical)

Calculate the weight of ASTM A182 F9 bar, plate or pipe →

Heat treatment, welding and machining

ItemUsual practice
Service temperature Up to ≈ 650 °C (ASME); oxidation limit ≈ 650 °C.
Heat treatment Full annealing or normalizing (≈ 950–1,000 °C) + subcritical tempering ≥ 675 °C.
Welding Air hardening: preheat 200–300 °C, consumable AWS E8018-B8 / E8015-B8 (A5.5), ER80S-B8 (A5.28); PWHT mandatory ≈ 730–790 °C. Do not use CE (IIW) as a criterion for 9Cr.
Machining Fair; harder than F11/F22 because of the higher hardness.

Plan an open-die forging in ASTM A182 F9: reduction, slenderness and how much material to send →Simulate the cutting plan of the ingot or bar →

Filler metal for welding

The wire composition is usually not identical to the material: each page explains why.

Typical applications

  • Refinery furnace flanges and fittings
  • Transfer lines of distillation and coking units
  • Valves for hot sulfidizing oil
  • High-temperature hydrogen service (Nelson curves)
  • Furnace and boiler tubes

Alternatives: F5 in less severe service at lower cost; F91 for creep and high pressure (higher strength); 316/317L stainless for naphthenic acids; 321/347 for severe H2S.

ASTM A182 F9: complete guide

What ASTM A182 F9 steel is

F9 is the grade with the highest chromium content among the conventional Cr-Mo alloy steels of ASTM A182, above F5 and F22. It is the forged version of A335 P9 pipe. Its density and weight are those of any steel; the advantage lies in resistance to oxidation and sulfur at high temperature, not in lightness or aqueous corrosion resistance.

Chemical composition and role of the elements

The 8 – 10% chromium forms a protective oxide layer stable up to about 650 °C; molybdenum increases creep resistance. Silicon, between 0.50 and 1.00%, reinforces oxidation resistance. Unlike F91, F9 has no vanadium, niobium or nitrogen, which is why its creep allowable stresses are much lower.

Mechanical properties

In the annealed or normalized and tempered condition the standard requires a minimum yield strength of 380 MPa, minimum tensile strength of 585 MPa, minimum elongation of 20%, minimum reduction of area of 40% and hardness between 179 and 217 HBW.

Heat treatment

Annealing or normalizing and tempering, with a minimum tempering temperature of 675 °C. Dustre performs the cycle in its own furnaces, with temperature records, as part of its heat treatment service.

Applications

Refinery and petrochemical furnaces, hot transfer lines, valves and flanges of hydrotreating and cracking units, heat exchangers with sulfurous fluids. For steam components in severe creep regime, F91 is the choice.

Supply forms and Dustre services

Round bars and blocks forged in open die, cut to size on a band saw, with rough or finish machining, heat treatment in our own furnaces and hardness, tensile and impact testing. All material is supplied with a 3.1 inspection certificate and heat traceability.

Frequently asked questions

What is the chemical composition of ASTM A182 F9?

Per ASTM A182/A182M – F9: C ≤ 0.15; Mn 0.30 – 0.60; P ≤ 0.030; S ≤ 0.030; Si 0.50 – 1.00; Cr 8.0 – 10.0.

Which standards cover ASTM A182 F9?

Forging (flanges, fittings, valves): ASTM A182/A182M F9; ASME SA-182. Larger forgings: ASTM A336 F9. Pipe/tube: ASTM A335 P9 / A213 T9. Plate: ASTM A387 Gr 9. Butt-welding fittings: ASTM A234 WP9. Casting: ASTM A217 C12.

Up to what temperature can ASTM A182 F9 be used?

Up to ≈ 650 °C (ASME); oxidation limit ≈ 650 °C.

Which materials can replace ASTM A182 F9?

F5 in less severe service at lower cost; F91 for creep and high pressure (higher strength); 316/317L stainless for naphthenic acids; 321/347 for severe H2S.

Where to buy ASTM A182 F9 in Brazil?

Dustre supplies ASTM A182 F9 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

Need ASTM A182 F9?Bars, forgings and parts with EN 10204 3.1 certificate.

Forms and stock of ASTM A182 F9

Dustre supplies ASTM A182 F9 as plate, pipe and tube, forgings and flanges, fittings and castings, cut to size, with forged and machined parts to drawing (shafts, discs, rings and blocks) and a 3.1 certificate.

Not in stock at the moment: supplied to order, with lead time in the quotation.

See the full ready-to-ship stock · Request a quote for ASTM A182 F9

Where to buy ASTM A182 F9 in Brazil?

Dustre supplies ASTM A182 F9 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

See also

HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp