ASTM A182 F22 / P22 – 2¼Cr-1Mo steel: standards, composition and properties

Download data sheet (PDF)

2¼Cr-1Mo is the most used chromium-molybdenum steel for high temperature and hydrogen service. The same composition gets different names depending on the product form: F22 for forgings, Gr 22 for plate, P22 and T22 for pipe and tube, WP22 for fittings and WC9 for castings. This page gathers all the standards, classes and treatments of the family.

Technical review Oct 2026 · * value to be confirmed in the current edition of the standard

UNSK21590
EN / W.Nr.1.7380 10CrMo9-10
Chromium2.00–2.50 %
Molybdenum0.87–1.13 %
Continuous serviceup to ≈ 595 °C
Density7.85 g/cm³

One composition, several standards

The name changes with the product form. When specifying, cite the standard, grade and class.

Standards for ASTM A182 F22 / P22 (2¼Cr-1Mo) by product form
FormASTM/ASMEGrade/classENABNT/others
Forging A182 / SA-182F22 Cl.1, F22 Cl.3EN 10222-2 11CrMo9-10 (1.7383)JIS G3203 SFVA F22*
Large forging A336 / SA-336F22 Cl.1, F22 Cl.3EN 10222-2 11CrMo9-10—
Quenched forging A508 / SA-508Gr 22 Cl.3 (also Cl.4, 5, 6 and 7)—Formerly A541 Gr 22 (withdrawn)
Plate A387 / SA-387Gr 22 Cl.1, Gr 22 Cl.2, Gr 22LEN 10028-2 10CrMo9-10 (1.7380)JIS G4109 SCMV4-1, SCMV4-2
Pipe A335 / SA-335P22EN 10216-2 10CrMo9-10JIS G3458 STPA24
Boiler tube A213 / SA-213T22EN 10216-2 10CrMo9-10JIS G3462 STBA24
Bar A739B22——
Butt-weld fittings A234 / SA-234WP22 Cl.1, WP22 Cl.3——
Casting A217 / SA-217WC9EN 10213 G17CrMo9-10 (1.7379)JIS G5151 SCPH32*
H₂S service NACE MR0175 / ISO 15156-2hardness ≤ 22 HRC—Reactor requirements: API RP 934-A

ASTM A541 was withdrawn and its grades, including Gr 22, were transferred to A508. "F22" alone does not define the strength: cite standard, grade and class.

Tolerances and HS codes

  • Forged bars (round and square): machining allowance from 2 mm (Ø 6–16 mm) to 24 mm (Ø 400–500 mm) on the diameter. E.g. Ø 100–125 mm finished: +7 mm, tolerance +6 / −0 (length up to 3,500 mm).
  • Forged discs: allowance of 4 to 9 mm on the diameter and 3 to 11 mm on the height, plus-only tolerance.
  • Cutting and machining: band saw −0 / +5 to +15 mm on length; waterjet +10 % of thickness on the diameter (min. 2 mm); machined parts −0 / +2 to +5 mm on the diameter. See the full tables (INF 002 and INF 003, the same for every alloy).
Tariff classification of ASTM A182 F22 / P22 (2¼Cr-1Mo): NCM, HS, HTS and CN by product form
FormNCM (Brazil, 8 digits)HS (international, 6 digits)HTS (USA, 10 digits)*CN (European Union, 8 digits)*
Forged bar7228.40.007228.407228.40.00007228 40 90
Hot-rolled bar7228.30.007228.307228.30.80417228 30 61
Plate (> 10 mm, width ≥ 600 mm)7225.40.907225.407225.40.30507225 40 40
Seamless pipe7304.19.007304.197304.19.50507304 19 10
Welded pipe7306.19.007306.197306.19.51507306 19 00
Flange and fitting7307.91.007307.917307.91.50307307 91 00

Tariff class: alloy steel (by chemical composition, under the Chapter 72 Notes and Section XV Note 5).

Pipe: 7304.19 and 7306.19 are line pipe for oil and gas pipelines; boiler, heat exchanger or process tubes go under 7304.39/7304.59 (seamless) and 7306.30/7306.50 (welded).

*: US and EU codes for reference. NCM per current legislation (General Rules of Interpretation, Notes to Chapters 72, 74 and 75 and Section XV Note 5). Confirm the final code with your customs broker according to the item size and finish. HS = first 6 digits of the NCM.

Chemical composition by standard (%)

The ranges of each standard side by side, to see where they differ.

Chemical composition of ASTM A182 F22 / P22 (2¼Cr-1Mo) by standard, in %
StandardCMnP maxS maxSi maxCrMoOthers
A182 F22 0.05–0.150.30–0.600.0400.0400.502.00–2.500.87–1.13—
A387 Gr 22 0.05–0.150.30–0.600.0250.0250.502.00–2.500.90–1.10Gr 22L: C ≤ 0.10
A335 P22 / A213 T22 0.05–0.150.30–0.600.0250.0250.501.90–2.600.87–1.13—
A234 WP22 0.05–0.150.30–0.600.0400.0400.501.90–2.60*0.87–1.13—
A217 WC9 0.05–0.180.40–0.700.04*0.045*0.602.00–2.750.90–1.20Cu ≤ 0.50; Ni ≤ 0.50; W ≤ 0.10; total ≤ 1.00
EN 10028-2 10CrMo9-10 0.08–0.140.40–0.800.0200.0100.502.00–2.500.90–1.10Cu ≤ 0.30
EN 10222-2 11CrMo9-10 0.08–0.150.40–0.800.0250.015*0.502.00–2.500.90–1.10Ni ≤ 0.30; Cu ≤ 0.30

Calculate the carbon equivalent of ASTM A182 F22 / P22 (2¼Cr-1Mo) for welding →

Mechanical properties by standard

Minimum values at room temperature, in the stated delivery condition.

Minimum mechanical properties of ASTM A182 F22 / P22 (2¼Cr-1Mo)
Standard and classYS minUTSElong.RAHardness
FORGINGS
A182 F22 Cl.1 205 MPa≥ 415 MPa20 %35 %≤ 170 HBW
A182 F22 Cl.3 310 MPa≥ 515 MPa20 %30 %156–207 HBW
A336 F22 Cl.1 205 MPa415–585 MPa20 %35 %*—
A336 F22 Cl.3 310 MPa515–690 MPa18 %45 %*—
A508 Gr 22 Cl.3 380 MPa585–760 MPa18 %45 %*—
ROLLED
A387 Gr 22 Cl.1 205 MPa415–585 MPa18 %40 %—
A387 Gr 22 Cl.2 310 MPa515–690 MPa18 %40 %—
EN 10028-2 10CrMo9-10 (≤ 16 mm) 310 MPa480–630 MPa18 %——
A335 P22 205 MPa≥ 415 MPa30 % long. / 20 % transv.——
A213 T22 205 MPa≥ 415 MPa30 %—≤ 163 HBW
EN 10216-2 10CrMo9-10 (≤ 40 mm) 280 MPa480–630 MPa22 % long.——
A739 B22 310 MPa515–655 MPa18 %——
FITTINGS AND CASTINGS
A234 WP22 Cl.1 205 MPa415–585 MPa20 %*—≤ 197 HBW
A234 WP22 Cl.3 310 MPa520–690 MPa20 %*—≤ 197 HBW
A217 WC9 275 MPa485–655 MPa20 %35 %—
EN 10213 G17CrMo9-10 +QT 400 MPa590–740 MPa18 %——

Calculate the weight of ASTM A182 F22 / P22 (2¼Cr-1Mo) bar, plate or pipe →

Class 1, Class 2 and Class 3: what changes

The composition is the same. The class defines the strength level obtained by heat treatment. Class 1 is annealed or normalized and tempered, with a minimum yield strength of 205 MPa. Class 3 of forgings and fittings, and Class 2 of plate, reach 310 MPa and are the most specified in steam and refinery projects. In A508, Classes 3, 4 and 5 are quenched and have even higher strength.

Heat treatments required by the standards

Delivery conditions and temperatures
StandardDelivery conditionMinimum tempering
A182 F22 Annealed, normalized and tempered, or quenched and tempered (austenitizing ≥ 900 °C)675 °C
A336 F22 Normalized or liquid quenched, followed by tempering675 °C
A508 Gr 22 Quenched (spray or immersion) and tempered, min. 0.5 h per inch650 °C
A387 Gr 22 Annealed or normalized and tempered; quenched and tempered by agreement675 °C*
A335 P22 / A213 T22 Full or isothermal anneal, or normalized and tempered675 °C
A234 WP22 Annealed, isothermally annealed or normalized and tempered675 °C
A739 B22 Normalized (927–982 °C) and tempered677 °C
A217 WC9 Normalized and tempered, or quenched and tempered675 °C
EN 10222-2 / 10028-2 +NT (normalized and tempered) or +QT (quenched and tempered)650–750 °C
JIS STPA24 / STBA24 Annealing or normalizing, followed by tempering650 °C

Plan an open-die forging in ASTM A182 F22 / P22 (2¼Cr-1Mo): reduction, slenderness and how much material to send →Simulate the cutting plan of the ingot or bar →

Variants in the family

Variants of ASTM A182 F22 / P22 (2¼Cr-1Mo)
VariantStandardsDifferenceYS / UTS
2¼Cr-1Mo-¼V (F22V, UNS K31835) A182 F22V, A336 F22V, A508 Gr 22V, A542 Type D Cl.4a, A832 22VV 0.25–0.35 %, C 0.11–0.15 %, controlled residuals; standard for modern reactors415 / 585–760 MPa
3Cr-1Mo (F21, UNS K31545) A182 F21, A336 F21, A387 Gr 21, A335 P21Cr 2.70–3.30 %; little used today310 / ≥ 515 MPa
Modified F22 (API 6A 75K) API 6A, based on A182 F22Adjusted chemistry and quench and temper up to class 75K; not an ASTM grade517 / ≥ 655 MPa
A387 Gr 22L A387Carbon ≤ 0.10 % for weldability and toughnessper class

Service temperature and hydrogen

  • Continuous use: up to about 565–595 °C; ASME II-D tabulates stresses up to 649 °C, but above 595 °C oxidation limits it.
  • Creep: starts to govern the design from about 425–480 °C.
  • Hydrogen (HTHA): on the Nelson curve (API RP 941), 2¼Cr-1Mo sits well above C-½Mo and 1¼Cr-½Mo; the vanadium version goes further.
  • Graphitization: does not occur: chromium stabilizes the carbides.
  • H₂S (NACE MR0175 / ISO 15156): accepted with hardness ≤ 22 HRC, including in the weld.

Temper embrittlement

  • Mechanism: in long service between about 370 and 565 °C, P, Sn, Sb and As segregate to the grain boundaries and raise the ductile-to-brittle transition temperature.
  • J factor (Watanabe), base metal: J = (Si + Mn) × (P + Sn) × 10⁴, in wt. %; usual limit J ≤ 100.
  • X̄ (Bruscato), weld metal: X̄ = (10P + 5Sb + 4Sn + As) / 100, in ppm; usual limit ≤ 15 ppm.
  • Step cooling: accelerated aging with Charpy curves before and after; the criterion comes from the purchaser's specification (API RP 934-A).

Welding

Usual welding practice
ItemUsual practice
Preheat 150 to 250 °C
Consumables AWS A5.5 E9018-B3 / E9015-B3 (electrode), A5.28 ER90S-B3 (TIG/MIG)
Post-weld heat treatment Mandatory, about 690 to 750 °C
Hydrogen in the weld Low-hydrogen consumables and post-heating to avoid cold cracking

Filler metal for welding

The wire composition is usually not identical to the material: each page explains why.

International equivalents

Equivalent designations
SystemDesignation
EN 10CrMo9-10 (1.7380) plate and pipe · 11CrMo9-10 (1.7383) forging · G17CrMo9-10 (1.7379) casting
Old DIN 10 CrMo 9 10 · GS-18 CrMo 9 10
Old AFNOR 10 CD 9.10
JIS SCMV4 (plate) · STPA24 (pipe) · STBA24 (boiler tube)
GB (China) 12Cr2Mo1R (plate) · 12Cr2MoG (tube)*

Equivalence is approximate: carbon, residuals and properties differ. Do not substitute one standard for another without a design review.

Typical applications

FormWhere it is used
Forging Flanges, nozzles and fittings for hydrotreating and hydrocracking reactors; forged rings and shells; steam and hydrogen flanges; F22 75K in API 6A wellheads
Plate Shells and heads of pressure vessels and reactors, boiler drums, high-pressure separators
Pipe P22: main and reheat steam, hydrogen lines · T22: superheaters, reheaters and exchangers
Fittings WP22 elbows, tees, reducers and caps matching P22 pipe
Casting Valve bodies and bonnets for steam and hydrogen, turbine and pump casings

Frequently asked questions

Are F22 and P22 the same steel?

Yes, the same 2¼Cr-1Mo family. F22 is the forging (A182) and P22 is the pipe (A335). The pipe has a slightly wider chromium range (1.90–2.60 %).

What is the difference between F11, F22 and F91?

F11 (1¼Cr-½Mo) serves lower temperatures. F22 withstands more creep and hydrogen. F91 (9Cr-1Mo-V) has much higher creep strength and allows thinner walls, but requires stricter welding and heat treatment.

When to order F22V instead of F22?

In large hydroprocessing reactors, where the higher strength of F22V reduces thickness and improves hydrogen resistance.

Can F22 be used in H₂S service?

Yes, per NACE MR0175 / ISO 15156, as long as the hardness stays at 22 HRC or below, including in the weld.

Need ASTM A182 F22 / P22 (2¼Cr-1Mo)?Bars, forgings and parts with EN 10204 3.1 certificate.

Forms and stock of ASTM A182 F22 / P22 (2¼Cr-1Mo)

Dustre supplies ASTM A182 F22 / P22 (2¼Cr-1Mo) as bar, plate, pipe and tube, forgings and flanges, fittings and castings, cut to size, with forged and machined parts to drawing (shafts, discs, rings and blocks) and a 3.1 certificate.

In stock in Osasco/SP, Brazil: round bar from Ø 30 to 350 mm. List updated on 11/13/2026.

See the full ready-to-ship stock · Request a quote for ASTM A182 F22 / P22 (2¼Cr-1Mo)

Where to buy ASTM A182 F22 / P22 (2¼Cr-1Mo) in Brazil?

Dustre supplies ASTM A182 F22 / P22 (2¼Cr-1Mo) as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

See also

HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp

We use your data only to answer this quote. Privacy. · WhatsApp +55 11 98649-0075 · Mon–Thu 07:00–17:00 · Fri 07:00–16:00 (Brasília time)