Dustre
EN
Customer area

ER80S-B8 – wire and rod for 9Cr-1Mo steel (F9)

9Cr-1Mo filler metal for ASTM A182 F9 forgings and tubes, used in refinery furnaces and high-temperature sulfur service.

Technical review Oct 2026 · composition per AWS A5.28/A5.28M; values marked * to be confirmed in the current edition of the standard

ClassificationER80S-B8
StandardAWS A5.28/A5.28M / ASME SFA-5.28
UNSS50480
GroupCr-Mo steel

Product forms and equivalents

ProcessClassification
TIG rod (GTAW) ER80S-B8
Solid MIG/MAG wire (GMAW) ER80S-B8
Covered electrode (SMAW) E8015-B8 / E8016-B8 / E8018-B8 – AWS A5.5
Submerged arc wire (SAW) EB8 + flux – AWS A5.23
Designations and equivalents
DesignationValue
AWS ER80S-B8
Specification AWS A5.28/A5.28M / ASME SFA-5.28
UNS S50480
Others EN ISO 21952-A: W/G CrMo9Si*; AWS A5.28M: ER55S-B8

Chemical composition (%)

AWS A5.28 (% by mass, filler metal)
Elementwt. %
C ≤ 0.10
Mn 0.40 – 0.70
Si ≤ 0.50
Cr 8.00 – 10.50
Mo 0.80 – 1.20
Ni ≤ 0.50
P ≤ 0.025
S ≤ 0.025
Cu ≤ 0.35

Properties of the deposited metal

PropertyValue
Tensile strength of deposited metal ≥ 550 MPa (AWS minimum, after PWHT)
Yield strength ≥ 470 MPa (AWS minimum, after PWHT)*
Elongation ≥ 17 % (AWS minimum, after PWHT)*

Materials welded with ER80S-B8

Why the composition differs from the base metal

As with F5, the wire limits carbon to 0.10 % so that the bead, which hardens in air, does not become excessively hard. Unlike F91, there is no addition of V, Nb and N; that is why it must not be used on F91.

Welding precautions

  • Preheat and interpass of about 200 to 300 °C.
  • PWHT typically between 705 and 760 °C.
  • Do not confuse with ER90S-B9, which is meant for F91.
  • TIG with pure argon; MIG/MAG with argon and 2–5 % O2 or up to 20 % CO2*. Clean, dry wire and bevel to limit hydrogen.

Frequently asked questions

What is ER80S-B8 used for?

9Cr-1Mo filler metal for ASTM A182 F9 forgings and tubes, used in refinery furnaces and high-temperature sulfur service.

Why is the composition of ER80S-B8 different from the material it welds?

As with F5, the wire limits carbon to 0.10 % so that the bead, which hardens in air, does not become excessively hard. Unlike F91, there is no addition of V, Nb and N; that is why it must not be used on F91.

Which covered electrode corresponds to ER80S-B8?

E8015-B8 / E8016-B8 / E8018-B8 – AWS A5.5.

What precautions apply when welding with ER80S-B8?

Preheat and interpass of about 200 to 300 °C. PWHT typically between 705 and 760 °C. Do not confuse with ER90S-B9, which is meant for F91. TIG with pure argon; MIG/MAG with argon and 2–5 % O2 or up to 20 % CO2*. Clean, dry wire and bevel to limit hydrogen.

Need ER80S-B8?Send the base material, the process and the wire or rod diameter.
HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp

We use your data only to answer this quote. Privacy. · WhatsApp +55 11 98649-0075 · Mon–Thu 07:00–17:00 · Fri 07:00–16:00 (Brasília time)