F138 stainless steel (316LVM) – UNS S31673

18Cr-14Ni-2.5Mo austenitic stainless steel for surgical implants

Download data sheet (PDF)

Variant of 316L with higher Ni and Mo, rigorous inclusion cleanliness and a fully austenitic microstructure (no delta ferrite), specified by ASTM F138 for implant bar and wire. Normally vacuum remelted (VAR) or ESR, hence the name 316LVM.

Technical review Oct 2026 · minimum values per the cited standard; physical properties are typical; values marked * to be confirmed in the standard

FamilyAustenitic stainless
UNSS31673
W.Nr. / EN1.4441 (X2CrNiMo18-15-3)
PREN≥ 26 (Cr + 3.3Mo, standard requirement)

Designations and equivalents

Designations of F138 stainless steel (316LVM) – UNS S31673
SystemDesignation
UNS S31673
W.Nr./EN 1.4441 (X2CrNiMo18-15-3)
DIN X2CrNiMo18-15-3
Trade names 316LVM
Others ISO 5832-1 (composition D); ASTM F139 (sheet)

Standards by product form

Standards for F138 stainless steel (316LVM) – UNS S31673
FormStandard
Bar and wire ASTM F138
Sheet and strip ASTM F139
Forging ASTM F621
International ISO 5832-1

Tolerances and HS codes

  • Forged bars (round and square): machining allowance from 2 mm (Ø 6–16 mm) to 24 mm (Ø 400–500 mm) on the diameter. E.g. Ø 100–125 mm finished: +7 mm, tolerance +6 / −0 (length up to 3,500 mm).
  • Forged discs: allowance of 4 to 9 mm on the diameter and 3 to 11 mm on the height, plus-only tolerance.
  • Cutting and machining: band saw −0 / +5 to +15 mm on length; waterjet +10 % of thickness on the diameter (min. 2 mm); machined parts −0 / +2 to +5 mm on the diameter. See the full tables (INF 002 and INF 003, the same for every alloy).
Tariff classification of F138 stainless steel (316LVM): NCM, HS, HTS and CN by product form
FormNCM (Brazil, 8 digits)HS (international, 6 digits)HTS (USA, 10 digits)*CN (European Union, 8 digits)*
Forged bar7222.30.007222.307222.30.00247222 30 51
Hot-rolled bar7222.11.007222.117222.11.00597222 11 11
Plate (> 10 mm, width ≥ 600 mm)7219.21.007219.217219.21.00207219 21 10
Flange and fitting7307.21.007307.217307.21.50007307 21 00

Tariff class: stainless steel (by chemical composition, under the Chapter 72 Notes and Section XV Note 5).

*: US and EU codes for reference. NCM per current legislation (General Rules of Interpretation, Notes to Chapters 72, 74 and 75 and Section XV Note 5). Confirm the final code with your customs broker according to the item size and finish. HS = first 6 digits of the NCM.

Chemical composition (%)

ASTM F138

Chemical composition of F138 stainless steel (316LVM) – UNS S31673, per ASTM F138
ElementRange (%)
C ≤ 0.030
Mn ≤ 2.00
P ≤ 0.025
S ≤ 0.010
Si ≤ 0.75
Cr 17.00 – 19.00
Ni 13.00 – 15.00
Mo 2.25 – 3.00
N ≤ 0.10
Cu ≤ 0.50
Fe balance
Cr + 3.3×Mo ≥ 26.0

Calculate the PREN of F138 stainless steel (316LVM) in the PREN calculator →

Mechanical properties

Annealed bar (ASTM F138); cold worked in parentheses

Mechanical properties of F138 stainless steel (316LVM) – UNS S31673
PropertyValue
Yield strength (0.2%) ≥ 190 MPa (cold worked: ≥ 690)
Tensile strength ≥ 490 MPa (cold worked: ≥ 860)
Elongation (4D) ≥ 40% (cold worked: ≥ 12%)
Extra hard (Ø 1.6 – 6.4 mm) Rm ≥ 1,350 MPa
Grain size ASTM 5 or finer
Inclusions (E45 A) ≤ 1.5 thin / ≤ 1.0 heavy

Typical physical properties

Typical values at 20 °C
PropertyValue
Density 8.0 g/cm³
Melting range ≈ 1,375 – 1,400 °C
Modulus of elasticity ≈ 193 – 200 GPa
Thermal conductivity (20 °C) ≈ 15 W/m·K (typical)
Thermal expansion (20–100 °C) ≈ 16 µm/m·K (typical)
Magnetic permeability non-magnetic (no delta ferrite)

Calculate the weight of F138 stainless steel (316LVM) bar, plate or pipe →

Heat treatment, welding and machining

ItemUsual practice
Service temperature Use at body temperature; not applicable to thermal service.
Heat treatment Supplied annealed (solution annealing ≈ 1,040 – 1,100 °C, rapid cooling) or cold worked according to the condition ordered. No delta ferrite, chi or sigma (ASTM E407, 100×).
Welding Normally not welded in implants. In instruments, TIG with high-purity ER316L (typical).
Machining Machinability lower than carbon steel: it work hardens quickly; use sharp tools, positive rake, constant feed without 'rubbing' and abundant coolant. Inclusion cleanliness reduces machinability compared with ordinary 316L.

Plan an open-die forging in F138 stainless steel (316LVM): reduction, slenderness and how much material to send →Simulate the cutting plan of the ingot or bar →

Filler metal for welding

The wire composition is usually not identical to the material: each page explains why.

Typical applications

  • Osteosynthesis plates and screws
  • Intramedullary nails and pins
  • Kirschner and cerclage wires
  • Steinmann pins and external fixators
  • Temporary trauma implants

Alternatives: Titanium Ti-6Al-4V ELI (ASTM F136) for permanent implants and better biocompatibility; high-N steel (ASTM F1586) when more strength is required; CoCrMo (F1537) in joint prostheses.

Compare alloys by corrosive medium, concentration and temperature →

F138 stainless steel (316LVM): complete guide

What ASTM F138 steel is

F138 is the number of the ASTM standard that specifies stainless steel bar and wire for surgical implants; the material itself has the designation UNS S31673 and is known as 316LVM (vacuum melted). It belongs to the family of austenitic stainless steels and derives from 316L, but with purity and microstructure requirements that industrial 316L does not meet.

Chemical composition and additional requirements

Chromium between 17 and 19%, nickel between 13 and 15% and molybdenum between 2.25 and 3.00%, with carbon up to 0.030%, sulfur up to 0.010% and phosphorus up to 0.025%. Besides the composition, the standard requires Cr + 3.3 × Mo of at least 26, ASTM grain size No. 5 or finer, inclusion limits per ASTM E45 and the absence of delta ferrite. Manganese is limited to 2%.

Mechanical properties by condition

Annealed, F138 has a minimum yield strength of 190 MPa, minimum tensile strength of 490 MPa and minimum elongation of 40%, and that 40% is a minimum, not a maximum. In the cold-worked condition, used in bone plates and screws, the minimums rise to 690 MPa yield and 860 MPa tensile, with a minimum elongation of 12%. In the extra-hard condition, for wires and thin rods, the minimum tensile strength is 1,350 MPa.

Corrosion and biocompatibility

The requirement Cr + 3.3 Mo ≥ 26 ensures pitting resistance in chloride-containing physiological fluid at 37 °C, and vacuum remelting reduces the inclusions that initiate pitting and fatigue cracks. F138 is indicated for temporary implants, such as osteosynthesis plates, screws and nails, and for instruments; permanent joint implants use titanium and cobalt-chromium alloys.

Applications

Osteosynthesis plates, screws, intramedullary nails and wires, external fixators, surgical and dental instruments, medical equipment components in contact with the body. For generic industrial use, ordinary 316L is the economical choice.

Supply forms and Dustre services

Round bars with an inspection certificate per ASTM F138 and heat traceability, band saw cutting to size and rough or finish machining.

Frequently asked questions

What is the chemical composition of F138 stainless steel (316LVM)?

Per ASTM F138: C ≤ 0.030; Mn ≤ 2.00; P ≤ 0.025; S ≤ 0.010; Si ≤ 0.75; Cr 17.00 – 19.00.

Which standards cover F138 stainless steel (316LVM)?

Bar and wire: ASTM F138. Sheet and strip: ASTM F139. Forging: ASTM F621. International: ISO 5832-1.

Up to what temperature can F138 stainless steel (316LVM) be used?

Use at body temperature; not applicable to thermal service.

Which materials can replace F138 stainless steel (316LVM)?

Titanium Ti-6Al-4V ELI (ASTM F136) for permanent implants and better biocompatibility; high-N steel (ASTM F1586) when more strength is required; CoCrMo (F1537) in joint prostheses.

Where to buy F138 stainless steel (316LVM) in Brazil?

Dustre supplies F138 stainless steel (316LVM) as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

Need F138 stainless steel (316LVM)?Bars, forgings and parts with EN 10204 3.1 certificate.

Forms and stock of F138 stainless steel (316LVM)

Dustre supplies F138 stainless steel (316LVM) as bar, plate and forgings and flanges, cut to size, with forged and machined parts to drawing (shafts, discs, rings and blocks) and a 3.1 certificate.

Not in stock at the moment: supplied to order, with lead time in the quotation.

See the full ready-to-ship stock · Request a quote for F138 stainless steel (316LVM)

Where to buy F138 stainless steel (316LVM) in Brazil?

Dustre supplies F138 stainless steel (316LVM) as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

See also

HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp

We use your data only to answer this quote. Privacy. · WhatsApp +55 11 98649-0075 · Mon–Thu 07:00–17:00 · Fri 07:00–16:00 (Brasília time)