Dustre
EN
Customer area

AISI 446 – UNS S44600

Oxidation-resistant 25% Cr ferritic stainless steel

Download data sheet (PDF)

Ferritic with 23–27% Cr and nitrogen, non-hardenable, with the highest oxidation and sulfidation resistance among ferritic stainless steels (up to ≈ 1,100 °C). It has low creep strength and limited toughness; it embrittles at 475 °C and by sigma phase on prolonged exposure.

Technical review Oct 2026 · minimum values per the cited standard; physical properties are typical; values marked * to be confirmed in the standard

FamilyFerritic stainless
UNSS44600
W.Nr. / EN≈ 1.4749 (X18CrN28; Cr 26–29%, approximate)
PREN≈ 25 – 31 (Cr + 16N)

Designations and equivalents

Designations of AISI 446 – UNS S44600
SystemDesignation
UNS S44600
W.Nr./EN ≈ 1.4749 (X18CrN28; Cr 26–29%, approximate)
DIN X18CrN28
JIS SUH446
Trade names Type 446
Others ISO X15CrN26; tubes A268 TP446-1 / TP446-2

Standards by product form

Standards for AISI 446 – UNS S44600
FormStandard
Bar ASTM A276 (446)
Plate ASTM A240 (446, on request); EN 10095 (1.4749)
Tube ASTM A268 TP446-1 / TP446-2
Forging ASTM A473 (446)

Tolerances and HS codes

  • Forged bars (round and square): machining allowance from 2 mm (Ø 6–16 mm) to 24 mm (Ø 400–500 mm) on the diameter. E.g. Ø 100–125 mm finished: +7 mm, tolerance +6 / −0 (length up to 3,500 mm).
  • Forged discs: allowance of 4 to 9 mm on the diameter and 3 to 11 mm on the height, plus-only tolerance.
  • Cutting and machining: band saw −0 / +5 to +15 mm on length; waterjet +10 % of thickness on the diameter (min. 2 mm); machined parts −0 / +2 to +5 mm on the diameter. See the full tables (INF 002 and INF 003, the same for every alloy).
Tariff classification of AISI 446: NCM, HS, HTS and CN by product form
FormNCM (Brazil, 8 digits)HS (international, 6 digits)HTS (USA, 10 digits)*CN (European Union, 8 digits)*
Forged bar7222.30.007222.307222.30.00247222 30 51
Hot-rolled bar7222.11.007222.117222.11.00597222 11 11
Plate (> 10 mm, width ≥ 600 mm)7219.21.007219.217219.21.00207219 21 10
Seamless pipe7304.41.907304.417304.41.60457304 41 00
Welded pipe7306.40.007306.407306.40.50857306 40 80
Flange and fitting7307.21.007307.217307.21.50007307 21 00

Tariff class: stainless steel (by chemical composition, under the Chapter 72 Notes and Section XV Note 5).

*: US and EU codes for reference. NCM per current legislation (General Rules of Interpretation, Notes to Chapters 72, 74 and 75 and Section XV Note 5). Confirm the final code with your customs broker according to the item size and finish. HS = first 6 digits of the NCM.

Chemical composition (%)

ASTM A276 (S44600)

Chemical composition of AISI 446 – UNS S44600, per ASTM A276 (S44600)
ElementRange (%)
C ≤ 0.20
Mn ≤ 1.50
Si ≤ 1.00
P ≤ 0.040
S ≤ 0.030
Cr 23.0 – 27.0
Ni ≤ 0.75
N 0.10 – 0.25
Fe balance

Calculate the PREN of AISI 446 in the PREN calculator →

Mechanical properties

Annealed (ASTM A276)

Mechanical properties of AISI 446 – UNS S44600
PropertyValue
Yield strength (0.2%) ≥ 275 MPa
Tensile strength ≥ 485 MPa
Elongation ≥ 20%
Hardness ≈ 160–210 HB (typical)

Typical physical properties

Typical values at 20 °C
PropertyValue
Density 7.50 g/cm³
Melting range 1,425 – 1,510 °C
Modulus of elasticity 200 GPa
Thermal conductivity (100 °C) 21.0 W/m·K
Thermal expansion (20–100 °C) 10.4 µm/m·K
Electrical resistivity 67 µΩ·cm

Calculate the weight of AISI 446 bar, plate or pipe →

Heat treatment, welding and machining

ItemUsual practice
Service temperature Oxidation: up to ≈ 1,100 °C continuous / 1,150 °C intermittent in air and sulfurous atmospheres. Low hot strength; avoid structural loads. Embrittlement at 400–540 °C (475 °C) and 540–870 °C (sigma).
Heat treatment Non-hardenable. Annealing 760–845 °C followed by rapid cooling (water or air) to avoid 475 °C embrittlement; stress relief after forming.
Welding Limited weldability (grain growth and low toughness in the HAZ). Preheat 150–230 °C, low heat input; anneal after welding when possible. Consumables AWS ER309/ER310 (tougher) or matching (ER446) when the oxidation resistance of the joint is critical.
Machining Fair; behavior similar to 430, with long chips and a tendency to smear.

Plan an open-die forging in AISI 446: reduction, slenderness and how much material to send →Simulate the cutting plan of the ingot or bar →

Filler metal for welding

The wire composition is usually not identical to the material: each page explains why.

Typical applications

  • Furnace components (supports, baskets, muffles)
  • Burners and radiant tubes
  • Recuperators and hot exchangers
  • Nozzles and blowing lances
  • Equipment in sulfurous atmospheres
  • Thermocouples (protection sheath)

Alternatives: AISI 310/310S when there is hot loading and toughness is required; 253 MA for creep; 430 or 409 for lower temperatures; nickel alloys (600/601) for severe cycling.

Compare alloys by corrosive medium, concentration and temperature →

AISI 446: complete guide

What AISI 446 stainless steel is

446 belongs to the family of martensitic and ferritic stainless steels, in the high-chromium ferritic group. With 23 to 27% chromium and at most 0.75% residual nickel, the structure is ferritic at all temperatures: the steel is magnetic, does not harden by quenching and owes its oxidation resistance to the chromium oxide layer that forms and regenerates up to about 1,100 °C.

Chemical composition and role of the elements

The high chromium ensures the protective layer in air, combustion gases and sulfur-bearing atmospheres; nitrogen, typically 0.10 to 0.25%, refines the grain and improves toughness; carbon up to 0.20% is the standard's ceiling, but commercial material usually has much less. There is no molybdenum, so pitting resistance in aqueous chlorides is limited despite the PREN of 25 to 31.

Applications

Burners and nozzles, thermowells, furnace supports, rails and baskets, heat recuperators, incinerator components, sulfurous gas ducts, heat treatment and foundry furnace parts in oxidizing atmospheres. In sulfur-bearing environments it is the alternative to high-nickel austenitics.

Supply forms and Dustre services

Round bars and blocks forged in open die, cut to size on a band saw, with rough or finish machining, heat treatment (quenching and tempering, annealing, solution annealing and aging) in our own furnaces and hardness, tensile and impact testing. All material is supplied with a 3.1 inspection certificate and heat traceability.

Frequently asked questions

What is the chemical composition of AISI 446?

Per ASTM A276 (S44600): C ≤ 0.20; Mn ≤ 1.50; Si ≤ 1.00; P ≤ 0.040; S ≤ 0.030; Cr 23.0 – 27.0.

Which standards cover AISI 446?

Bar: ASTM A276 (446). Plate: ASTM A240 (446, on request); EN 10095 (1.4749). Tube: ASTM A268 TP446-1 / TP446-2. Forging: ASTM A473 (446).

Up to what temperature can AISI 446 be used?

Oxidation: up to ≈ 1,100 °C continuous / 1,150 °C intermittent in air and sulfurous atmospheres. Low hot strength; avoid structural loads. Embrittlement at 400–540 °C (475 °C) and 540–870 °C (sigma).

Which materials can replace AISI 446?

AISI 310/310S when there is hot loading and toughness is required; 253 MA for creep; 430 or 409 for lower temperatures; nickel alloys (600/601) for severe cycling.

Is 446 stainless steel magnetic?

Yes. It is ferritic at all temperatures. Like other ferritic stainless steels, it can be used in soft magnetic components that need corrosion resistance, such as solenoid housings, cores and pole pieces, although its magnetic properties are inferior to those of conventional magnetic alloys. The relatively high electrical resistivity favors use in alternating current.

Does 446 resist sulfur-bearing atmospheres?

Yes. It is the ferritic stainless with the highest sulfidation resistance, up to ≈ 1,100 °C continuous in air and sulfurous atmospheres. It is the alternative to high-nickel austenitics, which suffer from sulfur.

Where to buy AISI 446 in Brazil?

Dustre supplies AISI 446 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

Need AISI 446?Bars, forgings and parts with EN 10204 3.1 certificate.

Forms and stock of AISI 446

Dustre supplies AISI 446 as bar, plate, pipe and tube and forgings and flanges, cut to size, with forged and machined parts to drawing (shafts, discs, rings and blocks) and a 3.1 certificate.

Not in stock at the moment: supplied to order, with lead time in the quotation.

See the full ready-to-ship stock · Request a quote for AISI 446

Where to buy AISI 446 in Brazil?

Dustre supplies AISI 446 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

See also

HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp