AISI 416 – UNS S41600

Free-machining (resulfurized) martensitic stainless steel

Download data sheet (PDF)

12–14% Cr stainless with sulfur ≥ 0.15% to form manganese sulfides, which makes it the most machinable stainless steel. Hardenable to ≈ 40 HRC; corrosion resistance is lower than 410 and all sulfur-free martensitic grades. There is no "416L" grade.

Technical review Oct 2026 · minimum values per the cited standard; physical properties are typical; values marked * to be confirmed in the standard

FamilyMartensitic stainless
UNSS41600
W.Nr. / EN1.4005 (X12CrS13)
PREN≈ 12 – 14

Designations and equivalents

Designations of AISI 416 – UNS S41600
SystemDesignation
UNS S41600
W.Nr./EN 1.4005 (X12CrS13)
DIN X12CrS13
JIS SUS416
Trade names Type 416
Others GB Y12Cr13 (formerly Y1Cr13); 416Se (S41623) with selenium

Standards by product form

Standards for AISI 416 – UNS S41600
FormStandard
Bar ASTM A582 (free-machining); AMS 5610; forging billet ASTM A314
Forging ASTM A473 (416)
Bar – general requirements ASTM A484
Wire ASTM A581

Tolerances and HS codes

  • Forged bars (round and square): machining allowance from 2 mm (Ø 6–16 mm) to 24 mm (Ø 400–500 mm) on the diameter. E.g. Ø 100–125 mm finished: +7 mm, tolerance +6 / −0 (length up to 3,500 mm).
  • Forged discs: allowance of 4 to 9 mm on the diameter and 3 to 11 mm on the height, plus-only tolerance.
  • Cutting and machining: band saw −0 / +5 to +15 mm on length; waterjet +10 % of thickness on the diameter (min. 2 mm); machined parts −0 / +2 to +5 mm on the diameter. See the full tables (INF 002 and INF 003, the same for every alloy).
Tariff classification of AISI 416: NCM, HS, HTS and CN by product form
FormNCM (Brazil, 8 digits)HS (international, 6 digits)HTS (USA, 10 digits)*CN (European Union, 8 digits)*
Forged bar7222.30.007222.307222.30.00247222 30 51
Hot-rolled bar7222.11.007222.117222.11.00597222 11 11
Flange and fitting7307.21.007307.217307.21.50007307 21 00

Tariff class: stainless steel (by chemical composition, under the Chapter 72 Notes and Section XV Note 5).

*: US and EU codes for reference. NCM per current legislation (General Rules of Interpretation, Notes to Chapters 72, 74 and 75 and Section XV Note 5). Confirm the final code with your customs broker according to the item size and finish. HS = first 6 digits of the NCM.

Chemical composition (%)

ASTM A582 (S41600)

Chemical composition of AISI 416 – UNS S41600, per ASTM A582 (S41600)
ElementRange (%)
C ≤ 0.15
Mn ≤ 1.25
Si ≤ 1.00
P ≤ 0.060
S ≥ 0.15
Cr 12.0 – 14.0
Mo ≤ 0.60 (optional)
Fe balance

Calculate the PREN of AISI 416 in the PREN calculator →

Mechanical properties

ASTM A582 controls hardness only (annealed ≤ 262 HB; condition T 248–302 HB; condition H 293–352 HB); typical tensile values

Mechanical properties of AISI 416 – UNS S41600
PropertyValue
Hardness, annealed (A582) ≤ 262 HB
Hardness, condition T / H (A582) 248–302 HB / 293–352 HB
Tensile strength (annealed, typ.) ≈ 517–620 MPa
Yield strength (annealed, typ.) ≈ 276–345 MPa
Elongation (annealed, typ.) ≈ 20–30%
Hardened (max.) ≈ 40 HRC

Typical physical properties

Typical values at 20 °C
PropertyValue
Density 7.75 g/cm³
Melting range 1,480 – 1,530 °C
Modulus of elasticity 200 GPa
Thermal conductivity (100 °C) 24.9 W/m·K
Thermal expansion (20–100 °C) 9.9 µm/m·K
Electrical resistivity 57 µΩ·cm

Calculate the weight of AISI 416 bar, plate or pipe →

Heat treatment, welding and machining

ItemUsual practice
Service temperature Not recommended for structural hot service; resists scaling up to ≈ 650 °C but loses strength, and the S promotes hot cracking.
Heat treatment Annealing 815–900 °C, slow furnace cool. Hardening: austenitize 925–1,010 °C, oil quench (small sections in air); temper right after (avoid 400–580 °C). Nitriding possible at 500–550 °C if tempering was done above that.
Welding Not recommended (S causes hot cracking). If unavoidable: preheat 200–300 °C and use AWS ER410 or ER309L/ER312, with post-weld tempering at 650–700 °C.
Machining Excellent: the most machinable stainless (≈ 85–90% of B1112), ideal for automatic lathes.

Plan an open-die forging in AISI 416: reduction, slenderness and how much material to send →Simulate the cutting plan of the ingot or bar →

Filler metal for welding

The wire composition is usually not identical to the material: each page explains why.

Typical applications

  • Automatic lathe parts (screws, nuts, pins)
  • Pump and motor shafts
  • Valve stems and internals
  • Light gears and bushings
  • Carburetor and instrument components

Alternatives: 410 or 403 when corrosion or welding matter; 420F for higher hardness; 303 for a non-magnetic free-machining stainless with better corrosion resistance; 17-4PH for high strength with good corrosion resistance.

Compare alloys by corrosive medium, concentration and temperature →

AISI 416: complete guide

Machining and anti-galling

Sulfur forms manganese sulfides that break the chip. Besides machining better than any other stainless, 416 has a low tendency to gall on threads and sliding surfaces. The price is corrosion resistance, lower than that of 403 and 410.

Corrosion

It resists moderate atmospheres, fresh water, steam, organic materials, mild acids and petroleum products, best in the quenched and tempered condition. Not suitable for chlorides. When corrosion outweighs machinability, the alternative is 410 or 403; with high strength, 17-4PH.

Hardening and nitriding

Small sections harden in air and larger ones in oil; hardness reaches ≈ 40 HRC depending on carbon and section. Quenched and tempered parts accept nitriding, but the nitrided case reduces corrosion resistance: use it only where the gain in wear justifies it.

Frequently asked questions

What is the chemical composition of AISI 416?

Per ASTM A582 (S41600): C ≤ 0.15; Mn ≤ 1.25; Si ≤ 1.00; P ≤ 0.060; S ≥ 0.15; Cr 12.0 – 14.0.

Which standards cover AISI 416?

Bar: ASTM A582 (free-machining); AMS 5610; forging billet ASTM A314. Forging: ASTM A473 (416). Bar – general requirements: ASTM A484. Wire: ASTM A581.

Up to what temperature can AISI 416 be used?

Not recommended for structural hot service; resists scaling up to ≈ 650 °C but loses strength, and the S promotes hot cracking.

Which materials can replace AISI 416?

410 or 403 when corrosion or welding matter; 420F for higher hardness; 303 for a non-magnetic free-machining stainless with better corrosion resistance; 17-4PH for high strength with good corrosion resistance.

Is there a 416L stainless steel?

No. There is no "416L" grade in the AISI/ASTM standards. The name appears commercially for AISI 416 itself (UNS S41600). When requesting a quote, confirm the standard (ASTM A582 or A479) and the composition.

Is 416 good for threads and sliding parts?

Yes. Sulfur reduces galling, which is why 416 is common in screws, nuts, bushings and valve stems. Avoid chloride-containing media.

Where to buy AISI 416 in Brazil?

Dustre supplies AISI 416 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

Need AISI 416?Bars, forgings and parts with EN 10204 3.1 certificate.

Forms and stock of AISI 416

Dustre supplies AISI 416 as bar and forgings and flanges, cut to size, with forged and machined parts to drawing (shafts, discs, rings and blocks) and a 3.1 certificate.

Not in stock at the moment: supplied to order, with lead time in the quotation.

See the full ready-to-ship stock · Request a quote for AISI 416

Where to buy AISI 416 in Brazil?

Dustre supplies AISI 416 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

See also

HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp

We use your data only to answer this quote. Privacy. · WhatsApp +55 11 98649-0075 · Mon–Thu 07:00–17:00 · Fri 07:00–16:00 (Brasília time)