ASTM A522 Type I – 9% Ni steel – UNS K81340

Forged 9% nickel ferritic steel for cryogenic service down to −196 °C

Download data sheet (PDF)

Low-carbon steel with 8.5–9.5% Ni, forged and rolled to ASTM A522/A522M for flanges, fittings and valves in cryogenic service. Supplied double normalized and tempered (NNT) or quenched and tempered (QT), it keeps its toughness at −196 °C and is the standard material for LNG tanks and lines.

Technical review Oct 2026 · minimum values per the cited standard; physical properties are typical; values marked * to be confirmed in the standard

FamilyAlloy steel
UNSK81340
W.Nr. / ENX8Ni9 – 1.5662 (EN 10222-3, forgings)

Designations and equivalents

Designations of ASTM A522 Type I – 9% Ni steel – UNS K81340
SystemDesignation
UNS K81340
W.Nr./EN X8Ni9 – 1.5662 (EN 10222-3, forgings)
DIN X8Ni9
JIS SL9N520 / SL9N590 (plate, JIS G3127)
Trade names 9% Ni, 9Ni
Others Plate A353/A553 Type I; pipe A333 Gr 8; fittings A420 WPL8

Standards by product form

Standards for ASTM A522 Type I – 9% Ni steel – UNS K81340
FormStandard
Forging (flanges, fittings, valves) ASTM A522/A522M Type I; ASME SA-522
Plate ASTM A353 (NNT) / A553 Type I (QT)
Pipe/tube ASTM A333 Gr 8 / A334 Gr 8
Butt-welding fittings ASTM A420 WPL8
EN bar/forging EN 10222-3 X8Ni9

Tolerances and HS codes

  • Forged bars (round and square): machining allowance from 2 mm (Ø 6–16 mm) to 24 mm (Ø 400–500 mm) on the diameter. E.g. Ø 100–125 mm finished: +7 mm, tolerance +6 / −0 (length up to 3,500 mm).
  • Forged discs: allowance of 4 to 9 mm on the diameter and 3 to 11 mm on the height, plus-only tolerance.
  • Cutting and machining: band saw −0 / +5 to +15 mm on length; waterjet +10 % of thickness on the diameter (min. 2 mm); machined parts −0 / +2 to +5 mm on the diameter. See the full tables (INF 002 and INF 003, the same for every alloy).
Tariff classification of ASTM A522 Type I: NCM, HS, HTS and CN by product form
FormNCM (Brazil, 8 digits)HS (international, 6 digits)HTS (USA, 10 digits)*CN (European Union, 8 digits)*
Forged bar7228.40.007228.407228.40.00007228 40 90
Hot-rolled bar7228.30.007228.307228.30.80417228 30 61
Plate (> 10 mm, width ≥ 600 mm)7225.40.907225.407225.40.30507225 40 40
Seamless pipe7304.19.007304.197304.19.50507304 19 10
Welded pipe7306.19.007306.197306.19.51507306 19 00
Flange and fitting7307.91.007307.917307.91.50307307 91 00

Tariff class: alloy steel (by chemical composition, under the Chapter 72 Notes and Section XV Note 5).

Pipe: 7304.19 and 7306.19 are line pipe for oil and gas pipelines; boiler, heat exchanger or process tubes go under 7304.39/7304.59 (seamless) and 7306.30/7306.50 (welded).

*: US and EU codes for reference. NCM per current legislation (General Rules of Interpretation, Notes to Chapters 72, 74 and 75 and Section XV Note 5). Confirm the final code with your customs broker according to the item size and finish. HS = first 6 digits of the NCM.

Chemical composition (%)

ASTM A522/A522M – Type I

Chemical composition of ASTM A522 Type I – 9% Ni steel – UNS K81340, per ASTM A522/A522M – Type I
ElementRange (%)
C ≤ 0.13
Mn ≤ 0.90
P ≤ 0.025
S ≤ 0.025
Si 0.15 – 0.30 (≤ 0.10 with vacuum deoxidation)
Ni 8.5 – 9.5

Calculate the carbon equivalent of ASTM A522 Type I – 9% Ni steel for welding →

Mechanical properties

NNT or QT – ASTM A522 Type I, room temperature

Mechanical properties of ASTM A522 Type I – 9% Ni steel – UNS K81340
PropertyValue
Yield strength (0.2%) ≥ 515 MPa
Tensile strength ≥ 690 MPa
Elongation ≥ 22%
Reduction of area ≥ 45%
Impact at −196 °C Charpy lateral expansion ≥ 0.38 mm

Typical physical properties

Typical values at 20 °C
PropertyValue
Density ≈ 7.86 g/cm³ (typical)
Modulus of elasticity ≈ 195 GPa (typical)

Calculate the weight of ASTM A522 Type I – 9% Ni steel bar, plate or pipe →

Heat treatment, welding and machining

ItemUsual practice
Service temperature −196 °C to 121 °C (scope of A522).
Heat treatment NNT: 900 °C in air + 790 °C in air + tempering 565–605 °C. QT: austenitize 800 ± 14 °C, water quench + tempering 565–605 °C. Cooling after tempering in air or water at ≥ 167 °C/h. Stress relief 550–585 °C.
Welding Weldable with nickel-based consumables (do not use ferritic consumables): AWS ENiCrMo-6 / ENiCrFe-9 (A5.11), ERNiMo-8 / ERNiCr-3 (A5.14). Control residual magnetism (arc blow) and heat input; PWHT normally waived per code.
Machining Similar to a 690 MPa low-alloy steel; good with carbide.

Plan an open-die forging in ASTM A522 Type I – 9% Ni steel: reduction, slenderness and how much material to send →Simulate the cutting plan of the ingot or bar →

Filler metal for welding

The wire composition is usually not identical to the material: each page explains why.

Typical applications

  • Flanges and fittings for LNG
  • Cryogenic valves
  • Tanks and lines for liquid nitrogen, oxygen and argon (down to −196 °C)
  • Regasification terminals and LNG carriers
  • Cryogenic vessel nozzles

Alternatives: A350 LF3 (3.5% Ni) down to −101 °C, cheaper; 304L/316L stainless (A182) when an austenitic without ductile-brittle transition is wanted; Invar 36 for low-expansion piping.

ASTM A522 Type I: complete guide

What ASTM A522 Type I steel is

A522 is the forged version of the 9% nickel steel of ASTM A353 and A553 plates. It belongs to the family of alloy steels, but with a function opposite to that of the Cr-Mo grades: instead of resisting heat, it keeps toughness at cryogenic temperatures at which ordinary carbon and low-alloy steels become brittle.

Chemical composition and role of nickel

Nickel (8.5 – 9.5%) lowers the ductile-brittle transition temperature and, with the correct heat treatment, produces a microstructure of tempered martensite with stable reverted austenite (formed during tempering), responsible for toughness at −196 °C. Carbon is kept low (≤ 0.13%) and phosphorus and sulfur are limited to 0.025% to preserve toughness.

Heat treatment

Double normalized and tempered or quenched and tempered, with tempering between 565 and 605 °C. Dustre performs the cycle in its own furnaces, with temperature records, as part of its heat treatment service, and confirms the result with impact testing.

Welding

The critical point of fabrication with 9% Ni is the consumable: welding must be done with a nickel alloy (ENiCrMo-6 / ERNiMo-8 or ENiCrMo-3), because ferritic consumables do not reach the toughness required at −196 °C. Preheating is unnecessary or low, and normally there is no post-weld heat treatment. The material is strongly magnetic, so parts must be demagnetized before welding.

Applications

Flanges, fittings, valves, nozzles and forged parts of LNG tanks and piping, air separation plants (liquid nitrogen and oxygen), ethylene and other liquefied gases, between −196 °C and about 120 °C.

Supply forms and Dustre services

Round bars and blocks forged in open die, cut to size on a band saw, with rough or finish machining, heat treatment in our own furnaces and hardness, tensile and impact testing. All material is supplied with a 3.1 inspection certificate and heat traceability.

Frequently asked questions

What is the chemical composition of ASTM A522 Type I?

Per ASTM A522/A522M – Type I: C ≤ 0.13; Mn ≤ 0.90; P ≤ 0.025; S ≤ 0.025; Si 0.15 – 0.30 (≤ 0.10 with vacuum deoxidation); Ni 8.5 – 9.5.

Which standards cover ASTM A522 Type I?

Forging (flanges, fittings, valves): ASTM A522/A522M Type I; ASME SA-522. Plate: ASTM A353 (NNT) / A553 Type I (QT). Pipe/tube: ASTM A333 Gr 8 / A334 Gr 8. Butt-welding fittings: ASTM A420 WPL8. EN bar/forging: EN 10222-3 X8Ni9.

Up to what temperature can ASTM A522 Type I be used?

−196 °C to 121 °C (scope of A522).

Which materials can replace ASTM A522 Type I?

A350 LF3 (3.5% Ni) down to −101 °C, cheaper; 304L/316L stainless (A182) when an austenitic without ductile-brittle transition is wanted; Invar 36 for low-expansion piping.

Why is A522 Type I used in cryogenic flanges and valves?

Nickel of 8.5 to 9.5%, with NNT or QT treatment, keeps toughness at −196 °C, a temperature at which ordinary carbon and low-alloy steels become brittle. That is why it is standard in LNG, liquid oxygen, nitrogen and argon.

Is A522 Type I suitable for high temperature?

No. The scope of ASTM A522 runs from −196 °C to 121 °C. For high temperature, use Cr-Mo steels such as F11 or F9 (ASTM A182).

Where to buy ASTM A522 Type I in Brazil?

Dustre supplies ASTM A522 Type I as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

Need ASTM A522 Type I?Bars, forgings and parts with EN 10204 3.1 certificate.

Forms and stock of ASTM A522 Type I

Dustre supplies ASTM A522 Type I as bar, plate, pipe and tube, forgings and flanges and fittings, cut to size, with forged and machined parts to drawing (shafts, discs, rings and blocks) and a 3.1 certificate.

Not in stock at the moment: supplied to order, with lead time in the quotation.

See the full ready-to-ship stock · Request a quote for ASTM A522 Type I

Where to buy ASTM A522 Type I in Brazil?

Dustre supplies ASTM A522 Type I as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

See also

HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp

We use your data only to answer this quote. Privacy. · WhatsApp +55 11 98649-0075 · Mon–Thu 07:00–17:00 · Fri 07:00–16:00 (Brasília time)