Naval brass C46400 – UNS C46400

Alpha-beta brass with tin for marine use

Download data sheet (PDF)

Brass with ≈ 60% Cu, 39% Zn and 0.5 – 1% Sn, where tin improves seawater corrosion resistance and dezincification resistance compared with common brass. Good strength, excellent hot formability and good forgeability. Used in shafts, marine hardware, condenser tubesheets and forged parts.

Technical review Oct 2026 · minimum values per the cited standard; physical properties are typical; values marked * to be confirmed in the standard

FamilyCopper and copper alloys
UNSC46400
W.Nr. / ENCW719R – CuZn39Sn1 (approx.)
Machinability (C36000 = 100)30
Forgeability (C37700 = 100)90

Designations and equivalents

Designations of Naval brass C46400 – UNS C46400
SystemDesignation
UNS C46400
W.Nr./EN CW719R – CuZn39Sn1 (approx.)
DIN 2.0530 – CuZn38Sn1 (approx.)*
JIS C4640
Trade names Naval brass, Tobin bronze*
Others AMS 4611, 4612; QQ-B-639; SAE J461/J463

Standards by product form

Standards for Naval brass C46400 – UNS C46400
FormStandard
Bar ASTM B21/B21M (bar, rod and shapes)
Forging ASTM B124/B124M, B283/B283M
Plate ASTM B171/B171M (condenser tubesheets)
Bar ASTM F467 / F468 (nuts and bolts)

Tolerances and HS codes

  • Forged bars (round and square): machining allowance from 2 mm (Ø 6–16 mm) to 24 mm (Ø 400–500 mm) on the diameter. E.g. Ø 100–125 mm finished: +7 mm, tolerance +6 / −0 (length up to 3,500 mm).
  • Forged discs: allowance of 4 to 9 mm on the diameter and 3 to 11 mm on the height, plus-only tolerance.
  • Cutting and machining: band saw −0 / +5 to +15 mm on length; waterjet +10 % of thickness on the diameter (min. 2 mm); machined parts −0 / +2 to +5 mm on the diameter. See the full tables (INF 002 and INF 003, the same for every alloy).
Tariff classification of Naval brass C46400: NCM, HS, HTS and CN by product form
FormNCM (Brazil, 8 digits)HS (international, 6 digits)HTS (USA, 10 digits)*CN (European Union, 8 digits)*
Forged bar7407.21.107407.217407.21.90007407 21 10
Hot-rolled bar7407.21.107407.217407.21.90007407 21 10
Plate (> 10 mm, width ≥ 600 mm)7409.29.007409.297409.29.00107409 29 00
Flange and fitting7412.20.007412.207412.20.00907412 20 00

Tariff class: copper-zinc alloy (brass) (by chemical composition, under the Chapter 72 Notes and Section XV Note 5).

*: US and EU codes for reference. NCM per current legislation (General Rules of Interpretation, Notes to Chapters 72, 74 and 75 and Section XV Note 5). Confirm the final code with your customs broker according to the item size and finish. HS = first 6 digits of the NCM.

Chemical composition (%)

ASTM B21 (UNS C46400)

Chemical composition of Naval brass C46400 – UNS C46400, per ASTM B21 (UNS C46400)
ElementRange (%)
Cu 59.0 – 62.0
Sn 0.50 – 1.0
Pb ≤ 0.20
Fe ≤ 0.10
Zn balance (Cu + named elements ≥ 99.6)

Mechanical properties

typical, bar (CDA)

Mechanical properties of Naval brass C46400 – UNS C46400
PropertyValue
Annealed (O60): tensile strength ≈ 395 MPa
Annealed (O60): yield strength (0.5%) ≈ 170 MPa
Annealed (O60): elongation ≈ 47%
Quarter hard (H01, Ø 25 mm): tensile strength ≈ 475 MPa
Quarter hard (H01, Ø 25 mm): yield strength (0.5%) ≈ 315 MPa
Quarter hard (H01, Ø 25 mm): elongation ≈ 27%
Hardness (H01) ≈ 75 – 80 HRB

Typical physical properties

Typical values at 20 °C
PropertyValue
Density 8.41 g/cm³
Melting range 888 – 899 °C
Modulus of elasticity 103 GPa
Electrical conductivity ≈ 26% IACS
Thermal conductivity (20 °C) ≈ 116 W/m·K
Thermal expansion (20–300 °C) 21.2 µm/m·K

Calculate the weight of Naval brass C46400 bar, plate or pipe →

Heat treatment, welding and machining

ItemUsual practice
Service temperature Usual use up to ≈ 200 °C*. In stagnant or hot seawater it may suffer dezincification; for those conditions, prefer copper-nickel or aluminum bronze.
Heat treatment Annealing at ≈ 425 – 595 °C. Hot working between ≈ 650 and 815 °C. Stress relief recommended after cold forming to reduce the risk of stress corrosion cracking*. Not hardenable by heat treatment.
Welding Excellent brazing and soft soldering; good oxyacetylene, spot and butt welding. TIG/MIG welding only fair because of zinc evaporation; covered electrode not recommended.
Machining Medium machinability (≈ 30, C36000 = 100). Continuous chip; sharp tool and chip breaker help.

Plan an open-die forging in Naval brass C46400: reduction, slenderness and how much material to send →Simulate the cutting plan of the ingot or bar →

Typical applications

  • Propeller shafts and rods for vessels
  • Marine hardware, nuts and bolts (ASTM F467/F468)
  • Condenser and heat exchanger tubesheets
  • Hot-forged parts for valves and fittings
  • Rings, bushings and structural components in marine environments

Alternatives: Nickel-aluminum bronze C63000 for higher strength and seawater corrosion resistance; 90/10 copper-nickel C70600 for piping and exchangers; common brass only in dry environments.

Frequently asked questions

What is the chemical composition of Naval brass C46400?

Per ASTM B21 (UNS C46400): Cu 59.0 – 62.0; Sn 0.50 – 1.0; Pb ≤ 0.20; Fe ≤ 0.10; Zn balance (Cu + named elements ≥ 99.6).

Which standards cover Naval brass C46400?

Bar: ASTM B21/B21M (bar, rod and shapes). Forging: ASTM B124/B124M, B283/B283M. Plate: ASTM B171/B171M (condenser tubesheets). Bar: ASTM F467 / F468 (nuts and bolts).

Up to what temperature can Naval brass C46400 be used?

Usual use up to ≈ 200 °C*. In stagnant or hot seawater it may suffer dezincification; for those conditions, prefer copper-nickel or aluminum bronze.

Which materials can replace Naval brass C46400?

Nickel-aluminum bronze C63000 for higher strength and seawater corrosion resistance; 90/10 copper-nickel C70600 for piping and exchangers; common brass only in dry environments.

Where to buy Naval brass C46400 in Brazil?

Dustre supplies Naval brass C46400 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

Need Naval brass C46400?Bars, forgings and parts with EN 10204 3.1 certificate.

Forms and stock of Naval brass C46400

Dustre supplies Naval brass C46400 as bar, plate and forgings and flanges, cut to size, with forged and machined parts to drawing (shafts, discs, rings and blocks) and a 3.1 certificate.

Not in stock at the moment: supplied to order, with lead time in the quotation.

See the full ready-to-ship stock · Request a quote for Naval brass C46400

Where to buy Naval brass C46400 in Brazil?

Dustre supplies Naval brass C46400 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

See also

HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp

We use your data only to answer this quote. Privacy. · WhatsApp +55 11 98649-0075 · Mon–Thu 07:00–17:00 · Fri 07:00–16:00 (Brasília time)