ASTM A182 F6NM – UNS S41500

Forged 13Cr-4Ni-Mo soft martensitic stainless steel (wrought equivalent of CA6NM)

Download data sheet (PDF)

F6NM is a low-carbon martensitic stainless with 3.5–5.5% Ni and 0.5–1.0% Mo, which after tempering forms reverted austenite and reaches high toughness, good weldability and cavitation resistance. It is the wrought equivalent of cast CA6NM, standard in hydraulic turbines, pumps and oil and gas valves.

Technical review Oct 2026 · minimum values per the cited standard; physical properties are typical; values marked * to be confirmed in the standard

FamilyMartensitic stainless
UNSS41500
W.Nr. / EN1.4313 (X3CrNiMo13-4)
PREN≈ 13 – 17

Designations and equivalents

Designations of ASTM A182 F6NM – UNS S41500
SystemDesignation
UNS S41500
W.Nr./EN 1.4313 (X3CrNiMo13-4)
DIN X3CrNiMo13-4
JIS SCS6 (cast, approximate)
Trade names 13-4, 13Cr4Ni, F6NM
Others Cast: ASTM A743/A487 CA6NM; AISI 415 (plate)

Standards by product form

Standards for ASTM A182 F6NM – UNS S41500
FormStandard
Forging/flange ASTM A182 / ASME SA-182 F6NM
Forging (vessels) ASTM A336 F6NM
Bar ASTM A479 / A276 (S41500)
Plate ASTM A240 (S41500)
Tube ASTM A268 (S41500)
Casting ASTM A743 / A487 CA6NM

Tolerances and HS codes

  • Forged bars (round and square): machining allowance from 2 mm (Ø 6–16 mm) to 24 mm (Ø 400–500 mm) on the diameter. E.g. Ø 100–125 mm finished: +7 mm, tolerance +6 / −0 (length up to 3,500 mm).
  • Forged discs: allowance of 4 to 9 mm on the diameter and 3 to 11 mm on the height, plus-only tolerance.
  • Cutting and machining: band saw −0 / +5 to +15 mm on length; waterjet +10 % of thickness on the diameter (min. 2 mm); machined parts −0 / +2 to +5 mm on the diameter. See the full tables (INF 002 and INF 003, the same for every alloy).
Tariff classification of ASTM A182 F6NM: NCM, HS, HTS and CN by product form
FormNCM (Brazil, 8 digits)HS (international, 6 digits)HTS (USA, 10 digits)*CN (European Union, 8 digits)*
Forged bar7222.30.007222.307222.30.00247222 30 51
Hot-rolled bar7222.11.007222.117222.11.00597222 11 11
Plate (> 10 mm, width ≥ 600 mm)7219.21.007219.217219.21.00207219 21 10
Seamless pipe7304.41.907304.417304.41.60457304 41 00
Welded pipe7306.40.007306.407306.40.50857306 40 80
Flange and fitting7307.21.007307.217307.21.50007307 21 00

Tariff class: stainless steel (by chemical composition, under the Chapter 72 Notes and Section XV Note 5).

*: US and EU codes for reference. NCM per current legislation (General Rules of Interpretation, Notes to Chapters 72, 74 and 75 and Section XV Note 5). Confirm the final code with your customs broker according to the item size and finish. HS = first 6 digits of the NCM.

Chemical composition (%)

ASTM A182 F6NM

Chemical composition of ASTM A182 F6NM – UNS S41500, per ASTM A182 F6NM
ElementRange (%)
C ≤ 0.05
Mn 0.50 – 1.00
Si ≤ 0.60
P ≤ 0.030
S ≤ 0.030
Cr 11.5 – 14.0
Ni 3.5 – 5.5
Mo 0.50 – 1.00
Fe balance

Calculate the PREN of ASTM A182 F6NM in the PREN calculator →

Mechanical properties

Quenched and tempered (ASTM A182 F6NM)

Mechanical properties of ASTM A182 F6NM – UNS S41500
PropertyValue
Yield strength (0.2%) ≥ 620 MPa
Tensile strength ≥ 790 MPa
Elongation ≥ 15%
Reduction of area ≥ 45%
Hardness ≤ 295 HB
H2S service (NACE MR0175) ≤ 23 HRC, double tempered

Typical physical properties

Typical values at 20 °C
PropertyValue
Density 7.70 g/cm³
Melting range ≈ 1,450 – 1,510 °C (typical)
Modulus of elasticity 200 GPa
Thermal conductivity (100 °C) ≈ 25 W/m·K (typical)
Thermal expansion (20–100 °C) ≈ 10.5 µm/m·K (typical)

Calculate the weight of ASTM A182 F6NM bar, plate or pipe →

Heat treatment, welding and machining

ItemUsual practice
Service temperature Structural use from ≈ −50 °C (with qualified Charpy) up to ≈ 350 °C.
Heat treatment Austenitize at 1,010 °C min., cool in air or liquid to below 95 °C; temper at 560–600 °C (ASTM A182). For NACE MR0175/ISO 15156: double tempering (≈ 670 °C + 600 °C) to ≤ 23 HRC.
Welding Good for a martensitic grade: preheat 100–150 °C, interpass ≤ 250 °C, post-weld treatment 580–620 °C. Consumables AWS E410NiMo-15/-16 and ER410NiMo.
Machining Fair to good in the tempered condition (≈ 250–290 HB); behavior close to hardened 410.

Plan an open-die forging in ASTM A182 F6NM: reduction, slenderness and how much material to send →Simulate the cutting plan of the ingot or bar →

Filler metal for welding

The wire composition is usually not identical to the material: each page explains why.

Typical applications

  • Hydraulic turbine runners and blades (Francis, Pelton, Kaplan)
  • Pump impellers and casings
  • O&G valve bodies, bonnets and internals
  • Water injection flanges and fittings
  • Compressors and subsea equipment
  • Parts subject to cavitation and erosion

Alternatives: 410/CA15 when toughness is not critical (cheaper); 431 for shafts with higher hardness; 17-4PH H1150D for higher strength; duplex 2205 (F51) when chlorides are present and the PREN of 13-4 is insufficient.

Compare alloys by corrosive medium, concentration and temperature →

ASTM A182 F6NM: complete guide

What F6NM stainless steel is

F6NM belongs to the family of martensitic and ferritic stainless steels, in the soft martensitic group (13Cr-4Ni). F6NM is the forging designation in ASTM A182; the material itself is UNS S41500, equivalent to the European 1.4313 and the cast CA6NM. Carbon limited to 0.05% and nickel of 3.5 to 5.5% produce a low-carbon martensite, tough and weldable, with a small fraction of retained austenite that absorbs impact. Molybdenum, from 0.5 to 1.0%, is mandatory in the standard and improves temper resistance and corrosion resistance.

Mechanical properties

Normalized and tempered, ASTM A182 requires a minimum yield strength of 620 MPa, minimum tensile strength of 790 MPa, minimum elongation of 15%, minimum reduction of area of 45% and maximum hardness of 295 HBW. For H2S service, NACE MR0175 / ISO 15156 requires double tempering and a hardness of up to 23 HRC.

Corrosion, cavitation and limits of use

With a PREN of 14 to 17, F6NM resists fresh water, wet steam and CO2-bearing media, but is limited in chlorides. Its advantage lies in resistance to cavitation and erosion, superior to the martensitic 410 and CA15 (the equivalent casting, CA6NM, performs similarly), which makes it the standard for Francis and Pelton runners and high-head pumps.

Applications

Hydraulic turbine runners, blades and shafts, high-pressure pump casings and impellers, valve stems and bodies, wellhead and compressor components, forged parts for the energy and oil and gas sectors.

Supply forms and Dustre services

Round bars and blocks forged in open die, cut to size on a band saw, with rough or finish machining, heat treatment (quenching and tempering, annealing, solution annealing and aging) in our own furnaces and hardness, tensile and impact testing. All material is supplied with a 3.1 inspection certificate and heat traceability.

Frequently asked questions

What is the chemical composition of ASTM A182 F6NM?

Per ASTM A182 F6NM: C ≤ 0.05; Mn 0.50 – 1.00; Si ≤ 0.60; P ≤ 0.030; S ≤ 0.030; Cr 11.5 – 14.0.

Which standards cover ASTM A182 F6NM?

Forging/flange: ASTM A182 / ASME SA-182 F6NM. Forging (vessels): ASTM A336 F6NM. Bar: ASTM A479 / A276 (S41500). Plate: ASTM A240 (S41500). Tube: ASTM A268 (S41500). Casting: ASTM A743 / A487 CA6NM.

Up to what temperature can ASTM A182 F6NM be used?

Structural use from ≈ −50 °C (with qualified Charpy) up to ≈ 350 °C.

Which materials can replace ASTM A182 F6NM?

410/CA15 when toughness is not critical (cheaper); 431 for shafts with higher hardness; 17-4PH H1150D for higher strength; duplex 2205 (F51) when chlorides are present and the PREN of 13-4 is insufficient.

Where to buy ASTM A182 F6NM in Brazil?

Dustre supplies ASTM A182 F6NM as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

Need ASTM A182 F6NM?Bars, forgings and parts with EN 10204 3.1 certificate.

Forms and stock of ASTM A182 F6NM

Dustre supplies ASTM A182 F6NM as bar, plate, pipe and tube, forgings and flanges and castings, cut to size, with forged and machined parts to drawing (shafts, discs, rings and blocks) and a 3.1 certificate.

In stock in Osasco/SP, Brazil: round bar from Ø 26 to 360 mm. List updated on 11/13/2026.

See the full ready-to-ship stock · Request a quote for ASTM A182 F6NM

Where to buy ASTM A182 F6NM in Brazil?

Dustre supplies ASTM A182 F6NM as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

See also

HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp

We use your data only to answer this quote. Privacy. · WhatsApp +55 11 98649-0075 · Mon–Thu 07:00–17:00 · Fri 07:00–16:00 (Brasília time)