S32205 / F60 duplex stainless steel: standards, composition and properties

1.4462

Download data sheet (PDF)

S32205 is the version of duplex 2205 with higher minimum chromium, molybdenum and nitrogen than S31803 (F51), which guarantees a minimum PREN of about 34. Like F51, it is 22Cr-5Ni-3Mo-N stainless with about half ferrite and half austenite, twice the yield strength of 316L and high resistance to chloride stress corrosion cracking. In forgings and flanges it is ASTM A182 F60; in plate, bar and pipe, S32205; in EN, 1.4462. Most plate, bar and pipe is dual-certified S31803/S32205.

Technical review Oct 2026 · * value to be confirmed in the current edition of the standard

UNSS32205 (wrought and forged); equivalent casting J92205
EN / W.Nr.1.4462 X2CrNiMoN22-5-3
Type22Cr austenitic-ferritic duplex stainless
YS / UTS min.450 / 655 MPa (wrought and forged)
PREN~34 at the standard minimum; ~35 typical
ASME temperatureMax. 316 °C; below −29 °C, with impact testing*

One composition, several standards

The name changes with the product form. When specifying, cite the standard, grade and class.

Standards for Duplex S32205 / F60 by product form
FormASTM/ASMEGrade/classENABNT/others
Plate, coil, strip A240 / SA-240S32205EN 10088-2, EN 10028-7 (1.4462)NORSOK M-630 MDS D45
Bar and section A276; A479 / SA-479S32205EN 10088-3; EN 10272 (1.4462)NORSOK M-630 MDS D47 (A479)
Forging and flange A182 / SA-182F60 (S32205)EN 10222-5, EN 10250-4* (1.4462)NORSOK MDS D44; ASME B16.5 group 2.8*
HIP part (powder metallurgy) A988 / SA-988S32205n/an/a
Seamless and welded pipe (piping) A790 / SA-790S32205EN 10216-5 (seamless), EN 10217-7 (welded)NORSOK MDS D41
Pipe welded with filler metal A928 / SA-928S32205n/aNORSOK MDS D42
Heat exchanger tube A789 / SA-789S32205EN 10216-5 (1.4462)NORSOK MDS D48
Welding fittings A815 / SA-815WPS32205 (CRS for MSS)EN 10253-4 (1.4462)NORSOK MDS D43
Casting A890 (general use); A995 / SA-995 (pressure)4A = CD3MN (J92205)EN 10213 / EN 10283: 1.4470 GX2CrNiMoN22-5-3NORSOK MDS D46
Welding consumable AWS A5.9 / A5.4 / A5.22ER2209, E2209-xx, E2209TxEN ISO 14343: 22 9 3 N LASME IX: P-No. 10H Gr 1
Detrimental phase testing A923Methods A, B, Cn/aISO 17781 (alternative used in O&G)

S32205 (F60) material meets orders for S31803 (F51), but not the other way around. Specify S32205 or F60 when the project requires a minimum PREN.

Tolerances and HS codes

  • Forged bars (round and square): machining allowance from 2 mm (Ø 6–16 mm) to 24 mm (Ø 400–500 mm) on the diameter. E.g. Ø 100–125 mm finished: +7 mm, tolerance +6 / −0 (length up to 3,500 mm).
  • Forged discs: allowance of 4 to 9 mm on the diameter and 3 to 11 mm on the height, plus-only tolerance.
  • Cutting and machining: band saw −0 / +5 to +15 mm on length; waterjet +10 % of thickness on the diameter (min. 2 mm); machined parts −0 / +2 to +5 mm on the diameter. See the full tables (INF 002 and INF 003, the same for every alloy).
Tariff classification of Duplex S32205 / F60: NCM, HS, HTS and CN by product form
FormNCM (Brazil, 8 digits)HS (international, 6 digits)HTS (USA, 10 digits)*CN (European Union, 8 digits)*
Forged bar7222.30.007222.307222.30.00247222 30 51
Hot-rolled bar7222.11.007222.117222.11.00597222 11 11
Plate (> 10 mm, width ≥ 600 mm)7219.21.007219.217219.21.00207219 21 10
Seamless pipe7304.41.907304.417304.41.60457304 41 00
Welded pipe7306.40.007306.407306.40.50857306 40 80
Flange and fitting7307.21.007307.217307.21.50007307 21 00

Tariff class: stainless steel (by chemical composition, under the Chapter 72 Notes and Section XV Note 5).

*: US and EU codes for reference. NCM per current legislation (General Rules of Interpretation, Notes to Chapters 72, 74 and 75 and Section XV Note 5). Confirm the final code with your customs broker according to the item size and finish. HS = first 6 digits of the NCM.

Chemical composition by standard (%)

The ranges of each standard side by side, to see where they differ.

Chemical composition of Duplex S32205 / F60 by standard, in %
StandardCMnP maxS maxSi maxCrNiMoNOthers
UNS S32205 (A240, A182 F60, A790) 0.0302.000.0300.0201.0022.0–23.04.5–6.53.0–3.50.14–0.20n/a
A890 / A995 4A (CD3MN, J92205) 0.0301.500.0400.0201.0021.0–23.54.5–6.52.5–3.50.10–0.30Cu 1.00
EN 1.4462 X2CrNiMoN22-5-3 (EN 10088, EN 10216-5) 0.0302.000.0350.0151.0021.0–23.04.5–6.52.5–3.50.10–0.22*n/a
EN 1.4470 GX2CrNiMoN22-5-3 (cast) 0.0302.000.0350.0251.0021.0–23.04.5–6.52.5–3.50.12–0.20n/a
AISI 329 / S32900 (comparison, NOT 2205) 0.081.000.0400.0300.7523.0–28.02.0–5.01.0–2.0not specifiedn/a

Calculate the PREN of Duplex S32205 / F60 in the PREN calculator →

Mechanical properties by standard

Minimum values at room temperature, in the stated delivery condition.

Minimum mechanical properties of Duplex S32205 / F60
Standard and conditionYS minUTSElong.RAHardness
FORGINGS
A182 F60 (S32205), solution annealed 450 MPa (65 ksi)655 MPa min (95 ksi)25 %45 %not specified in the table
ROLLED
A240 S32205, solution-annealed plate 450 MPa (65 ksi)655 MPa min (95 ksi)25 %n/a293 HBW / 31 HRC max
A479 / A276 S32205, bar 450 MPa655 MPa min25 %n/a290 HBW max
EN 10088-2 1.4462, quarto plate (P) 460 MPa640–840 MPa25 %n/an/a
EN 10088-3 1.4462, bar 450 MPa650–880 MPa25 %n/a270 HB max
PIPE, FITTINGS AND CASTINGS
A790 / A789 S32205, pipe/tube 450 MPa655 MPa min25 %n/a290 HBW max
A815 WPS32205, fitting 450 MPa655 MPa min20 %n/a290 HBW max
EN 10216-5 1.4462, seamless pipe 450 MPa640–880 MPa22 %*n/aKV 40 J at -40 °C*
A890 / A995 4A (CD3MN), cast 415 MPa (60 ksi)*620 MPa min (90 ksi)25 %n/an/a
EN 10213 1.4470, cast 420 MPa600–800 MPa20 %n/an/a

Calculate the weight of Duplex S32205 / F60 bar, plate or pipe →

F60 (S32205) vs. F51 (S31803): what is the difference

S31803 is the original designation of 22Cr duplex; with the wide Cr, Mo and N ranges (N min. 0.08 %), a heat could come out with a PREN near 30. S32205 was created to pin 2205 at the top of the range: Cr 22.0–23.0, Mo 3.0–3.5 and N 0.14–0.20, minimum PREN ~34, and a higher minimum UTS (655 vs. 620 MPa). Almost all plate, bar and pipe today ships dual-certified S31803/S32205. S32205 (F60) material can be accepted where S31803 (F51) is ordered, but not the other way around.

Heat treatments required by the standards

Delivery conditions and temperatures
StandardDelivery conditionTemperature
A240 / A790 / A789 (S32205) Solution annealed + rapid cooling (water or other fast medium)1020–1100 °C (1870–2010 °F)
A182 F60 Solution annealed + quenched in liquid (water), cooled below 260 °C1020–1100 °C (1870–2010 °F)
A276 / A479 Solution annealed + rapid cooling1020 °C min*
A815 WPS32205 Solution annealed + water quenched (mandatory after forming/welding)1020–1100 °C
A890 / A995 4A Solution annealed + water quenched; or furnace cool to ≥ 1010 °C, hold 15 min and water quench1120 °C min (2050 °F)
EN 10088 / EN 10216-5 (1.4462) Solution annealed (+AT) + water or forced air1020–1100 °C

Plan an open-die forging in Duplex S32205 / F60: reduction, slenderness and how much material to send →Simulate the cutting plan of the ingot or bar →

Variants in the family

Variants of Duplex S32205 / F60
VariantStandardsDifferenceYS / UTS
S31803 / F51 A240, A479, A790, A182 F51Original range: Cr 21–23, Mo 2.5–3.5, N 0.08–0.20450 / 620 MPa
S32205 / F60 A240, A479, A790, A182 F60Restricted range: Cr 22–23, Mo 3.0–3.5, N 0.14–0.20; min. PREN ~34450 / 655 MPa
Cast 4A (CD3MN, J92205) A890, A995, EN 1.4470Mn 1.50 max, N up to 0.30, Cu 1.00; higher solution annealing415 / 620 MPa
Lean duplex 2304 (S32304) / 2101 (S32101) A240, A790Little or no Mo; cheaper, PREN ~24–26 (does not replace 2205 in chlorides)*400–450 / 600–650 MPa*
Super duplex 2507 (S32750, F53) A240, A182 F53, A790, A995 5A25Cr-7Ni-4Mo-0.3N; PREN ≥ 40, for seawater550 / 795 MPa
AISI 329 (S32900) A240, A789/A790Old 25Cr-2/5Ni-1.5Mo duplex without controlled N; NOT equivalent to 2205485 / 620 MPa

Corrosion, PREN and temperature

  • PREN (Cr + 3.3 Mo + 16 N): ~35 typical; at the standard minimum, ~34 for S32205 (for S31803/F51, ~30.5).
  • Pitting and crevice corrosion: CPT in 6 % FeCl3 (ASTM G48) typically 35 to 45 °C. Good in moderate chlorides; for natural seawater use super duplex.
  • Chloride stress corrosion cracking: far superior to 304/316L austenitics, one of the main reasons for its use.
  • Temperature: ASME (II-D) limits use to 316 °C (600 °F); below −29 °C (−20 °F) the code requires Charpy impact testing*. Above ~300 °C, 475 °C embrittlement (alpha prime phase) occurs; mills limit it to 350 °C.
  • Sigma and nitrides: precipitate in the ~700–950 °C range* in poorly cooled solution anneals, high-heat-input welds or thick sections; they collapse toughness and pitting resistance (see A923).
  • NACE MR0175 / ISO 15156-3: solution annealed and rapidly cooled, 35–65 % ferrite, no hardness limit; accepted up to 232 °C with pH2S ≤ 10 kPa (0.1 bar). NACE MR0103: up to 28 HRC.

Compare alloys by corrosive medium, concentration and temperature →

Tests required for duplex (ASTM A923, G48)

  • A923 Method A: NaOH etch and metallographic examination for intermetallic phases; used only for acceptance (a poor result leads to Method B or C).
  • A923 Method B (Charpy): -40 °C; min. 54 J (40 ft-lbf) in base metal and HAZ, 34 J (25 ft-lbf) in weld metal (S32205, J92205).
  • A923 Method C (FeCl3): 25 °C for base metal and 22 °C for weld, 24 h, max. loss 10 mdd (1.0 g/m²). There is no criterion for the J92205 casting in this table.
  • ASTM G48: Method A (pitting) or E (CPT) in 6 % FeCl3; the temperature and criterion come from the project or from NORSOK, not from G48. O&G projects usually accept up to 4.0 g/m² in welds*.
  • NORSOK M-630 / ISO 17781: besides G48, they require low-temperature Charpy and ferrite content in qualification; values per the MDS and project revision*.
  • Ferrite measurement: ferrite control (typically 35–65 % in base metal and 30–70 % in weld*) is required in O&G and sour service.

Welding

Usual welding practice
ItemUsual practice
Consumable ER2209 (AWS A5.9), E2209-15/16/17 (A5.4), E2209T0/T1 (A5.22); EN ISO 14343 22 9 3 N L. Higher Ni than the base metal to balance ferrite.
ASME IX classification P-No. 10H, Group 1
Preheat Not needed (only dry the part)
Interpass 150 °C max (100 °C in thin sections or by project requirement)*
Heat input ~0.5–2.5 kJ/mm; up to 1–3 kJ/mm with a qualified procedure. Too low gives excess ferrite, too high gives sigma.
Gas TIG: Ar or Ar + 2 % N2; root purge with Ar or Ar + N2
PWHT No stress relief is done; only full solution annealing when the standard requires it (e.g. A815 fittings)

Filler metal for welding

The wire composition is usually not identical to the material: each page explains why.

International equivalents

Equivalent designations
SystemDesignation
UNS S32205; equivalent casting J92205
ASTM forging F60 (S32205)
ASTM casting Grade 4A / CD3MN (A890, A995)
EN / W.Nr. X2CrNiMoN22-5-3 / 1.4462; cast GX2CrNiMoN22-5-3 / 1.4470
JIS No exact equivalent (SUS329J3L is closer to S31803 / F51)
GB 022Cr23Ni5Mo3N (S22053)
BS / AFNOR / SIS (old) 318S13 / Z3CND22-05Az / SS 2377
ABNT No designation in NBR 5601: specify by UNS and ASTM standard
Trade names SAF 2205 (Alleima), Forta DX 2205 (Outokumpu), ATI 2205, UR 45N

SUS329J3L (JIS) has Cr up to 24 % and N min. 0.08 %, so it is closer to S31803 (F51), not S32205. No "329" designation without the J3L suffix corresponds to 2205.

Typical applications

Form or industryWhere it is used
Offshore oil and gas Process piping, manifolds, F60 flanges, vessels and separators
Chemicals and petrochemicals Heat exchangers (A789), tanks, chloride-bearing lines
Pulp and paper Digesters, liquor and bleaching tanks
Chemical tankers Cargo tanks and heating coils
Pumps and valves Cast 4A bodies, shafts and stems in A479 bar
Water and sanitation Desalination (parts not exposed to hot seawater), effluent piping
Structures Bridges, fasteners and structures where the high YS is used to reduce thickness

Frequently asked questions

Is F60 quench hardened?

No. Duplex stainless steel does not harden by quenching. The "quench" in ASTM A182 is only the rapid cooling after solution annealing, in water, to below 260 °C. It keeps the ferrite/austenite balance and prevents sigma and chi phases. Strength and hardness come from the chemistry and hot working, not from heat treatment.

Is 2205 the same as 329 or '329A' stainless?

No. AISI 329 (UNS S32900) is an old 23–28Cr duplex with 1–2 % Mo and no specified nitrogen. '329A' is not a recognized UNS, ASTM or JIS designation. The confusion comes from the Japanese SUS329J3L, which is the JIS equivalent of 2205. When buying, order by UNS S31803/S32205 or F51/F60.

Is F60 the same as 2205?

Yes. F60 is the ASTM A182 forging of S32205, today’s 2205. F51 is S31803, the original designation, with a wider composition range. F60 material meets F51 orders, but F51 does not meet F60.

What is the difference between A890 4A and A995 4A?

The composition (CD3MN) is the same. A890 is for general-purpose castings; A995 is for pressure parts (valves, pumps) and enters ASME as SA-995.

Up to what temperature can I use 2205?

ASME limits S32205 to 316 °C (600 °F) because of 475 °C embrittlement. At low temperature, common use goes down to about -40/-50 °C with proven Charpy values.

Need Duplex S32205 / F60?Bars, forgings and parts with EN 10204 3.1 certificate.

Forms and stock of Duplex S32205 / F60

Dustre supplies Duplex S32205 / F60 as bar, plate, pipe and tube, forgings and flanges, fittings and castings, cut to size, with forged and machined parts to drawing (shafts, discs, rings and blocks) and a 3.1 certificate.

In stock in Osasco/SP, Brazil: plate from 10 to 25.4 mm and round bar from Ø 31.75 to 406.4 mm. List updated on 11/13/2026.

See the full ready-to-ship stock · Request a quote for Duplex S32205 / F60

Where to buy Duplex S32205 / F60 in Brazil?

Dustre supplies Duplex S32205 / F60 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

See also

HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp

We use your data only to answer this quote. Privacy. · WhatsApp +55 11 98649-0075 · Mon–Thu 07:00–17:00 · Fri 07:00–16:00 (Brasília time)