Dustre
EN
Customer area

Chromium copper C18200 – UNS C18200

Precipitation-hardening copper with ≈ 1% Cr

Download data sheet (PDF)

Copper with 0.6 – 1.2% chromium, precipitation hardenable, offering ≈ 80% IACS conductivity and tensile strength of ≈ 450 – 530 MPa in the aged condition. It keeps much of its hardness at moderate temperatures, which is why it is used in welding electrodes and electrical parts that heat up. Contains no beryllium.

Technical review Oct 2026 · minimum values per the cited standard; physical properties are typical; values marked * to be confirmed in the standard

FamilyCopper and copper alloys
UNSC18200
W.Nr. / ENCW105C – CuCr1
Machinability (C36000 = 100)20

Designations and equivalents

Designations of Chromium copper C18200 – UNS C18200
SystemDesignation
UNS C18200
W.Nr./EN CW105C – CuCr1
DIN 2.1291 (CuCr)
Trade names CuCr1, RWMA Class 2
Others MIL-C-19311 (forgings, bar and strip)

Standards by product form

Standards for Chromium copper C18200 – UNS C18200
FormStandard
Bar MIL-C-19311; EN 12163 (CW105C)*
Forging MIL-C-19311; EN 12420 (CW105C)*
Wire ASTM F9

Tolerances and HS codes

  • Forged bars (round and square): machining allowance from 2 mm (Ø 6–16 mm) to 24 mm (Ø 400–500 mm) on the diameter. E.g. Ø 100–125 mm finished: +7 mm, tolerance +6 / −0 (length up to 3,500 mm).
  • Forged discs: allowance of 4 to 9 mm on the diameter and 3 to 11 mm on the height, plus-only tolerance.
  • Cutting and machining: band saw −0 / +5 to +15 mm on length; waterjet +10 % of thickness on the diameter (min. 2 mm); machined parts −0 / +2 to +5 mm on the diameter. See the full tables (INF 002 and INF 003, the same for every alloy).
Tariff classification of Chromium copper C18200: NCM, HS, HTS and CN by product form
FormNCM (Brazil, 8 digits)HS (international, 6 digits)HTS (USA, 10 digits)*CN (European Union, 8 digits)*
Forged bar7407.10.107407.107407.10.50507407 10 00
Hot-rolled bar7407.10.107407.107407.10.50507407 10 00
Flange and fitting7412.10.007412.107412.10.00007412 10 00

Tariff class: refined copper (by chemical composition, under the Chapter 72 Notes and Section XV Note 5). Copper alloyed with chromium (and zirconium) within the limits of Chapter 74 Note 1 a) counts as refined copper.

*: US and EU codes for reference. NCM per current legislation (General Rules of Interpretation, Notes to Chapters 72, 74 and 75 and Section XV Note 5). Confirm the final code with your customs broker according to the item size and finish. HS = first 6 digits of the NCM.

Chemical composition (%)

CDA / UNS C18200

Chemical composition of Chromium copper C18200 – UNS C18200, per CDA / UNS C18200
ElementRange (%)
Cr 0.6 – 1.2
Fe ≤ 0.10
Si ≤ 0.10
Pb ≤ 0.05
Cu balance (Cu + named elements ≥ 99.5)

Mechanical properties

typical, bar (CDA)

Mechanical properties of Chromium copper C18200 – UNS C18200
PropertyValue
Solution treated (TB00): tensile strength ≈ 310 MPa
Aged (TF00, Ø 25 mm): tensile strength ≈ 495 MPa
Aged (TF00, Ø 25 mm): yield strength (0.5%) ≈ 450 MPa
Aged (TF00, Ø 25 mm): elongation ≈ 18%
Cold worked and aged (TH04): tensile strength ≈ 530 MPa
Hardness, aged ≈ 70 – 82 HRB

Typical physical properties

Typical values at 20 °C
PropertyValue
Density 8.89 g/cm³
Melting range 1,070 – 1,075 °C
Modulus of elasticity 117 GPa
Electrical conductivity (aged) ≈ 80% IACS
Thermal conductivity (20 °C) ≈ 324 W/m·K
Thermal expansion (20–100 °C) 17.6 µm/m·K

Calculate the weight of Chromium copper C18200 bar, plate or pipe →

Heat treatment, welding and machining

ItemUsual practice
Service temperature Begins to soften above ≈ 450 °C*; for hotter service, prefer chromium-zirconium copper C18150.
Heat treatment Solution treatment at ≈ 1,000 – 1,030 °C with rapid cooling. Aging at ≈ 460 °C for ≈ 3 h, air cooling. Hot working between ≈ 815 and 925 °C.
Welding Good brazing and soft soldering. TIG/MIG welding possible, with loss of hardening in the affected zone. Spot, seam and oxyacetylene welding not recommended.
Machining Low machinability (≈ 20, C36000 = 100). Sharp tool, positive rake and coolant; best in the aged condition.

Plan an open-die forging in Chromium copper C18200: reduction, slenderness and how much material to send →Simulate the cutting plan of the ingot or bar →

Typical applications

  • Electrodes and electrode holders for resistance welding
  • Contacts, terminals and busbars that run hot
  • Circuit breaker and switch components
  • Welding machine parts and conductive clamps
  • Molds and components needing heat transfer

Alternatives: Chromium-zirconium copper C18150 for a higher softening temperature and electrode life; low-beryllium copper C17510 when more hardness is needed.

Frequently asked questions

What is the chemical composition of Chromium copper C18200?

Per CDA / UNS C18200: Cr 0.6 – 1.2; Fe ≤ 0.10; Si ≤ 0.10; Pb ≤ 0.05; Cu balance (Cu + named elements ≥ 99.5).

Which standards cover Chromium copper C18200?

Bar: MIL-C-19311; EN 12163 (CW105C)*. Forging: MIL-C-19311; EN 12420 (CW105C)*. Wire: ASTM F9.

Up to what temperature can Chromium copper C18200 be used?

Begins to soften above ≈ 450 °C*; for hotter service, prefer chromium-zirconium copper C18150.

Which materials can replace Chromium copper C18200?

Chromium-zirconium copper C18150 for a higher softening temperature and electrode life; low-beryllium copper C17510 when more hardness is needed.

Where to buy Chromium copper C18200 in Brazil?

Dustre supplies Chromium copper C18200 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

Need Chromium copper C18200?Bars, forgings and parts with EN 10204 3.1 certificate.

Forms and stock of Chromium copper C18200

Dustre supplies Chromium copper C18200 as bar and forgings and flanges, cut to size, with forged and machined parts to drawing (shafts, discs, rings and blocks) and a 3.1 certificate.

Not in stock at the moment: supplied to order, with lead time in the quotation.

See the full ready-to-ship stock · Request a quote for Chromium copper C18200

Where to buy Chromium copper C18200 in Brazil?

Dustre supplies Chromium copper C18200 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

See also

HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp

We use your data only to answer this quote. Privacy. · WhatsApp +55 11 98649-0075 · Mon–Thu 07:00–17:00 · Fri 07:00–16:00 (Brasília time)