Beryllium copper C17200

Precipitation-hardening copper alloy (≈ 2% Be)

Download data sheet (PDF)

The strongest copper alloy: after aging it exceeds 1,200 MPa and about 38 – 42 HRC, while keeping electrical conductivity around 22% IACS. Combines high fatigue resistance, good corrosion resistance and the absence of sparking and magnetism. Supplied solution treated (soft, for machining and forming) or already hardened.

Technical review Oct 2026 · minimum values per the cited standard; physical properties are typical; values marked * to be confirmed in the standard

FamilyCopper and copper alloys
UNSC17200
W.Nr. / ENCW101C – CuBe2
Machinability (C36000 = 100)20

Designations and equivalents

Designations of Beryllium copper C17200 – UNS C17200
SystemDesignation
UNS C17200
W.Nr./EN CW101C – CuBe2
DIN 2.1247 (CuBe2)
JIS C1720
Trade names Alloy 25 (Materion), Berylco 25 (NGK), CuBe2
Others AMS 4533, 4534, 4650, 4651; MIL-C-21657; SAE J461/J463

Standards by product form

Standards for Beryllium copper C17200 – UNS C17200
FormStandard
Bar ASTM B196/B196M
Plate ASTM B194 (plate, strip and rolled bar)
Forging ASTM B570 (forgings and extrusions)
Wire ASTM B197/B197M*

Tolerances and HS codes

  • Forged bars (round and square): machining allowance from 2 mm (Ø 6–16 mm) to 24 mm (Ø 400–500 mm) on the diameter. E.g. Ø 100–125 mm finished: +7 mm, tolerance +6 / −0 (length up to 3,500 mm).
  • Forged discs: allowance of 4 to 9 mm on the diameter and 3 to 11 mm on the height, plus-only tolerance.
  • Cutting and machining: band saw −0 / +5 to +15 mm on length; waterjet +10 % of thickness on the diameter (min. 2 mm); machined parts −0 / +2 to +5 mm on the diameter. See the full tables (INF 002 and INF 003, the same for every alloy).
Tariff classification of Beryllium copper C17200: NCM, HS, HTS and CN by product form
FormNCM (Brazil, 8 digits)HS (international, 6 digits)HTS (USA, 10 digits)*CN (European Union, 8 digits)*
Forged bar7407.29.107407.297407.29.50007407 29 00
Hot-rolled bar7407.29.107407.297407.29.50007407 29 00
Plate (> 10 mm, width ≥ 600 mm)7409.90.007409.907409.90.10307409 90 00
Flange and fitting7412.20.007412.207412.20.00907412 20 00

Tariff class: other copper alloys (beryllium copper) (by chemical composition, under the Chapter 72 Notes and Section XV Note 5).

*: US and EU codes for reference. NCM per current legislation (General Rules of Interpretation, Notes to Chapters 72, 74 and 75 and Section XV Note 5). Confirm the final code with your customs broker according to the item size and finish. HS = first 6 digits of the NCM.

Chemical composition (%)

ASTM B196 / B194 (UNS C17200)

Chemical composition of Beryllium copper C17200 – UNS C17200, per ASTM B196 / B194 (UNS C17200)
ElementRange (%)
Be 1.80 – 2.00
Co + Ni ≥ 0.20
Co + Ni + Fe ≤ 0.6
Al ≤ 0.20
Si ≤ 0.20
Pb ≤ 0.02
Cu balance (Cu + named elements ≥ 99.5)

Mechanical properties

typical, bar (CDA)

Mechanical properties of Beryllium copper C17200 – UNS C17200
PropertyValue
Solution treated (TB00): tensile strength ≈ 495 MPa
Aged (TF00): tensile strength ≈ 1,255 MPa
Aged (TF00): yield strength (0.2%) ≈ 1,000 – 1,200 MPa
Aged (TF00): elongation ≈ 3 – 4%
Cold worked and aged (TH04): tensile strength ≈ 1,345 – 1,415 MPa
Hardness, aged (TF00 / TH04) ≈ 39 – 42 HRC
Fatigue strength (10⁸ cycles, TF00) ≈ 380 MPa

Typical physical properties

Typical values at 20 °C
PropertyValue
Density 8.26 g/cm³
Melting range 866 – 982 °C
Modulus of elasticity 128 GPa
Electrical conductivity (aged) ≈ 22% IACS
Thermal conductivity (20 °C) ≈ 107 – 130 W/m·K
Thermal expansion (20–300 °C) 17.8 µm/m·K

Calculate the weight of Beryllium copper C17200 bar, plate or pipe →

Heat treatment, welding and machining

ItemUsual practice
Service temperature Recommended up to ≈ 150 – 200 °C in continuous service under load; above that it loses strength by overaging and stress relaxation*. Keeps toughness at cryogenic temperatures.
Heat treatment Solution treatment at ≈ 775 – 800 °C with water quench. Precipitation hardening at ≈ 315 °C for 2 – 3 h, air cooling. Hot working between ≈ 650 and 815 °C. Stress relief at ≈ 200 °C.
Welding Good brazing and soft soldering on a clean surface. TIG/MIG and spot welding possible; the affected zone loses its hardening and the part must be heat treated again. Oxyacetylene welding not recommended. Caution: dry machining, grinding and sanding generate beryllium-containing dust; work with coolant and local exhaust.
Machining Machines best in the aged, or solution treated and cold worked, condition; annealed it is gummy. Sharp carbide tool and abundant coolant. Caution: dry machining, grinding and sanding generate beryllium-containing dust; work with coolant and local exhaust.

Plan an open-die forging in Beryllium copper C17200: reduction, slenderness and how much material to send →Simulate the cutting plan of the ingot or bar →

Typical applications

  • Highly stressed springs, electrical contacts and connectors
  • Non-sparking tools for explosive atmospheres
  • Bushings and bearings for high loads (landing gear, heavy equipment)
  • Plastic injection mold inserts with fast cooling
  • Non-magnetic instrument and well-drilling components
  • High-strength fasteners and Belleville washers

Alternatives: Low-beryllium copper C17510 when conductivity matters more than strength; chromium-zirconium copper C18150 for electrodes and conductive parts; nickel-aluminum bronze C63000 for beryllium-free bushings and non-sparking tools, with lower strength.

Frequently asked questions

What is the chemical composition of Beryllium copper C17200?

Per ASTM B196 / B194 (UNS C17200): Be 1.80 – 2.00; Co + Ni ≥ 0.20; Co + Ni + Fe ≤ 0.6; Al ≤ 0.20; Si ≤ 0.20; Pb ≤ 0.02.

Which standards cover Beryllium copper C17200?

Bar: ASTM B196/B196M. Plate: ASTM B194 (plate, strip and rolled bar). Forging: ASTM B570 (forgings and extrusions). Wire: ASTM B197/B197M*.

Up to what temperature can Beryllium copper C17200 be used?

Recommended up to ≈ 150 – 200 °C in continuous service under load; above that it loses strength by overaging and stress relaxation*. Keeps toughness at cryogenic temperatures.

Which materials can replace Beryllium copper C17200?

Low-beryllium copper C17510 when conductivity matters more than strength; chromium-zirconium copper C18150 for electrodes and conductive parts; nickel-aluminum bronze C63000 for beryllium-free bushings and non-sparking tools, with lower strength.

Where to buy Beryllium copper C17200 in Brazil?

Dustre supplies Beryllium copper C17200 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

Need Beryllium copper C17200?Bars, forgings and parts with EN 10204 3.1 certificate.

Forms and stock of Beryllium copper C17200

Dustre supplies Beryllium copper C17200 as bar, plate and forgings and flanges, cut to size, with forged and machined parts to drawing (shafts, discs, rings and blocks) and a 3.1 certificate.

Not in stock at the moment: supplied to order, with lead time in the quotation.

See the full ready-to-ship stock · Request a quote for Beryllium copper C17200

Where to buy Beryllium copper C17200 in Brazil?

Dustre supplies Beryllium copper C17200 as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

See also

HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp

We use your data only to answer this quote. Privacy. · WhatsApp +55 11 98649-0075 · Mon–Thu 07:00–17:00 · Fri 07:00–16:00 (Brasília time)