PET-C (Ertalyte®) – semi-crystalline polyester, natural and PTFE-filled

The engineering plastic with the highest dimensional stability and low wear in humid environments

Download data sheet (PDF)

Semi-crystalline PET is the most dimensionally stable engineering plastic: it absorbs very little water, has low thermal expansion and excellent wear resistance. It outperforms POM and nylon in precision parts that run wet. The PTFE-filled grade (Ertalyte TX, TECAPET TF) lowers friction for bushings and guides without lubrication.

Technical review Oct 2026 · typical values from semi-finished stock manufacturers' catalogues (23 °C, ISO/ASTM methods stated), not specification minimums; values with * to be confirmed

FamilyThermoplastic polyester
Continuous temperature115 / 100 °C
Dynamic frictionPET-C: 0.2 · PET + PTFE: 0.19

Designations and equivalents

Designations of PET-C (Ertalyte®) – semi-crystalline polyester, natural and PTFE-filled
SystemDesignation
Abbreviation (ISO 1043) PET-C / PET + PTFE
Trade names Ertalyte (MCAM); TECAPET (Ensinger); Ertalyte TX (MCAM); TECAPET TF grey (Ensinger)

Standards by product form

Standards for PET-C (Ertalyte®) – semi-crystalline polyester, natural and PTFE-filled
FormStandard
Rod, sheet and tube Manufacturer's specification (MCAM Ertalyte, Ensinger TECAPET)
Food contact FDA 21 CFR 177.1630; EU 10/2011
Machined part to drawing ISO 2768 tolerance or as per drawing

Composition and filler

Nominal composition

Composition of PET-C (Ertalyte®) – semi-crystalline polyester, natural and PTFE-filled
ComponentContent
Semi-crystalline PET 100% (natural) or with PTFE
PTFE-filled grade PTFE incorporated as a solid lubricant

Mechanical properties

Typical values from the stock-shape manufacturer's catalog, 23 °C (PET-C, PET + PTFE); ISO/ASTM methods as per the source

Mechanical properties of PET-C (Ertalyte®) – semi-crystalline polyester, natural and PTFE-filled
PropertyValue
Tensile strength PET-C: 90 MPa · PET + PTFE: 76 MPa
Modulus of elasticity (tensile) PET-C: 3,500 MPa · PET + PTFE: 3,300 MPa
Elongation at break PET-C: 15% · PET + PTFE: 5%
Compressive strength PET-C: 103 MPa · PET + PTFE: 102 MPa
Hardness PET-C: Rockwell M 96 · PET + PTFE: Rockwell M 94
Notched impact PET-C: 2 kJ/m² · PET + PTFE: 2.5 kJ/m²

Typical physical and thermal properties

Typical values at 23 °C unless stated
PropertyValue
Density PET-C: 1.39 g/cm³ · PET + PTFE: 1.44 g/cm³
Maximum continuous service temperature 115 / 100 °C
Maximum short-term temperature 160 °C
Minimum service temperature -20 °C
HDT (1.8 MPa) PET-C: 80 °C · PET + PTFE: 75 °C
Melting point or glass transition 245 °C
Linear thermal expansion PET-C: 80 µm/m·K · PET + PTFE: 85 µm/m·K
Thermal conductivity 0.29 W/m·K
Water absorption (24 h) PET-C: 0.07 / 0.16% · PET + PTFE: 0.06 / 0.13%
Water absorption (saturation) PET-C: 0.5% · PET + PTFE: 0.47%
Dielectric strength PET-C: 22 kV/mm · PET + PTFE: 21 kV/mm
Flammability (UL 94) HB

Calculate the weight of PET-C (Ertalyte®) – semi-crystalline polyester, natural and PTFE-filled bar, plate or pipe →

Friction, wear and PV limit

Friction and wear of PET-C (Ertalyte®) – semi-crystalline polyester, natural and PTFE-filled
PropertyValue
Dynamic coefficient of friction against steel PET-C: 0.2 (dynamic, dry against steel (MCAM QTM 55007)) · PET + PTFE: 0.19 (dynamic, dry against steel (MCAM QTM 55007))
PV limit (pressure × velocity) PET-C: 0.098 MPa·m/s (MCAM QTM 55007, dry against steel, safety factor 4:1 already applied; original 2,800 psi·ft/min) · PET + PTFE: 0.21 MPa·m/s (MCAM QTM 55007, dry against steel, safety factor 4:1 already applied; original 6,000 psi·ft/min)

PV and friction depend on the test method, the mating surface (steel, stainless, roughness), lubrication and each manufacturer's safety factor: compare values from the same source and confirm by testing in critical applications.

Chemical resistance

Chemical resistance of PET-C (Ertalyte®) – semi-crystalline polyester, natural and PTFE-filled at room temperature (guidance only; check concentration and temperature)
MediumResistance
Acids Limited in strong acids; good in weak acids
Bases (alkalis) Limited: bases and hot water above 60 °C hydrolyze PET
Solvents Good (ketones/esters acceptable); chlorinated solvents unacceptable
Hydrocarbons and oils Very good
Steam and hot water Limited (hydrolysis above ~60 °C)

Compare PET-C (Ertalyte®) – semi-crystalline polyester, natural and PTFE-filled with the other plastics by application, temperature and medium →

Stock forms and sizes

  • Rod (round bar)
  • Sheet (plate)
  • Tube and bushing
  • Raw material: rod (round bar), sheet (plate) and tube, cut to size
  • Machined part to drawing or sample, in the same order as the metal parts
  • Lot certificate of conformity; FDA/EU 10/2011 declaration when the grade allows

Service temperature, machining and assembly

ItemUsual practice
Service temperature Continuous service up to 115 / 100 °C, short peaks up to 160 °C; minimum -20 °C (unloaded; under load, limited by HDT and creep).
Annealing (stress relief) Stress-relief annealing before precision machining.
Bonding and welding Bonding is possible after surface preparation.
Machining Machines very well, with excellent stability and surface finish.

Typical applications

  • Precision parts for food and packaging machinery
  • Bushings, guides and wear strips
  • Pistons and valves
  • Instrument and fixture parts

Alternatives: POM for lower cost; PEEK for higher temperature and steam.

Frequently asked questions

Which standards cover PET-C (Ertalyte®)?

Rod, sheet and tube: Manufacturer's specification (MCAM Ertalyte, Ensinger TECAPET). Food contact: FDA 21 CFR 177.1630; EU 10/2011. Machined part to drawing: ISO 2768 tolerance or as per drawing.

Up to what temperature can PET-C (Ertalyte®) be used?

Continuous service up to 115 / 100 °C, short peaks up to 160 °C; minimum -20 °C (unloaded; under load, limited by HDT and creep).

Which materials can replace PET-C (Ertalyte®)?

POM for lower cost; PEEK for higher temperature and steam.

PET or POM?

PET is more dimensionally stable and wears less; POM is tougher and cheaper. In precision parts running wet, PET usually wins.

Where to buy PET-C (Ertalyte®) in Brazil?

Dustre supplies PET-C (Ertalyte®) as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

Need PET-C (Ertalyte®)?Rods, sheets, tubes and parts machined to drawing, with lot certificate of conformity.

Forms and stock of PET-C (Ertalyte®)

Dustre supplies PET-C (Ertalyte®) as bar, plate and pipe and tube, cut to size, with forged and machined parts to drawing (shafts, discs, rings and blocks) and a 3.1 certificate.

Not in stock at the moment: supplied to order, with lead time in the quotation.

See the full ready-to-ship stock · Request a quote for PET-C (Ertalyte®)

Where to buy PET-C (Ertalyte®) in Brazil?

Dustre supplies PET-C (Ertalyte®) as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

See also

HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp

We use your data only to answer this quote. Privacy. · WhatsApp +55 11 98649-0075 · Mon–Thu 07:00–17:00 · Fri 07:00–16:00 (Brasília time)