PAI (Torlon® 4301) – polyamide-imide

The strongest thermoplastic up to 260 °C, bearing grade with PTFE and graphite

Download data sheet (PDF)

Polyamide-imide is the thermoplastic with the highest strength and stiffness up to about 260 °C, with very low creep. Grade 4301, with PTFE and graphite, is made for bearings and wear rings under high load and speed. It absorbs some moisture, which changes dimensions: precision parts require dry, stabilized material.

Technical review Oct 2026 · typical values from semi-finished stock manufacturers' catalogues (23 °C, ISO/ASTM methods stated), not specification minimums; values with * to be confirmed

FamilyHigh-performance polymer
Continuous temperature260 °C
Density1.45 g/cm³
Dynamic friction0.2

Designations and equivalents

Designations of PAI (Torlon® 4301) – polyamide-imide
SystemDesignation
Abbreviation (ISO 1043) PAI
Trade names Torlon 4301 (Syensqo/Solvay, resin); Duratron T4301 PAI (MCAM); TECAPAI CM XP440 (Ensinger)

Standards by product form

Standards for PAI (Torlon® 4301) – polyamide-imide
FormStandard
Rod, tube and sheet Manufacturer's specification (Solvay Torlon; MCAM Duratron T4301)
Machined part to drawing ISO 2768 tolerance or as per drawing

Composition and filler

Nominal composition of the bearing grade

Composition of PAI (Torlon® 4301) – polyamide-imide
ComponentContent
PAI (polyamide-imide) ≈ 85%
PTFE + graphite ≈ 15% (grade 4301)*

Mechanical properties

Typical values from the stock-shape manufacturer's catalog, 23 °C; ISO/ASTM methods as per the source

Mechanical properties of PAI (Torlon® 4301) – polyamide-imide
PropertyValue
Tensile strength 103 MPa
Modulus of elasticity (tensile) 6,210 MPa
Elongation at break 3%
Compressive strength 152 MPa
Hardness Rockwell M 106
Notched impact 42.7 J/m

Typical physical and thermal properties

Typical values at 23 °C unless stated
PropertyValue
Density 1.45 g/cm³
Maximum continuous service temperature 260 °C
Maximum short-term temperature 270 °C
Minimum service temperature -20 °C
HDT (1.8 MPa) 279 °C
Melting point or glass transition 275 °C
Linear thermal expansion 25.2 µm/m·K
Thermal conductivity 0.533 W/m·K
Water absorption (24 h) 0.4%
Water absorption (saturation) 1.5%
Flammability (UL 94) V-0

Calculate the weight of PAI (Torlon® 4301) – polyamide-imide bar, plate or pipe →

Friction, wear and PV limit

Friction and wear of PAI (Torlon® 4301) – polyamide-imide
PropertyValue
Dynamic coefficient of friction against steel 0.2 (dynamic, dry against steel (MCAM QTM 55007))
PV limit (pressure × velocity) 1.4 MPa·m/s (MCAM QTM 55007, dry against steel, safety factor 4:1 already applied; original 40,000 psi·ft/min; requires post-cure); 0.326 MPa·m/s (ASTM D3702 (Ensinger USA), no safety factor stated; original 9,300 psi·ft/min (compression molded))

PV and friction depend on the test method, the mating surface (steel, stainless, roughness), lubrication and each manufacturer's safety factor: compare values from the same source and confirm by testing in critical applications.

Chemical resistance

Chemical resistance of PAI (Torlon® 4301) – polyamide-imide at room temperature (guidance only; check concentration and temperature)
MediumResistance
Acids Limited in strong acids; good in weak acids
Bases (alkalis) Poor (strong alkalis unacceptable)
Solvents Good (including chlorinated solvents, ketones, esters)
Hydrocarbons and oils Good
Steam and hot water Limited (absorbs water; steam above ~150 °C degrades it)

Compare PAI (Torlon® 4301) – polyamide-imide with the other plastics by application, temperature and medium →

Stock forms and sizes

  • Rod (round bar)
  • Tube and bushing
  • Sheet (plate)
  • Raw material: rod (round bar), sheet (plate) and tube, cut to size
  • Machined part to drawing or sample, in the same order as the metal parts
  • Lot certificate of conformity; FDA/EU 10/2011 declaration when the grade allows

Service temperature, machining and assembly

ItemUsual practice
Service temperature Continuous service up to 260 °C, short peaks up to 270 °C; minimum -20 °C (unloaded; under load, limited by HDT and creep).
Annealing (stress relief) The material is supplied already post-cured by the manufacturer; anneal only as instructed by the manufacturer.
Bonding and welding Bonding with epoxy after surface preparation.
Machining Machines with carbide tooling; store dry before machining precision parts.

Typical applications

  • Bearings and wear rings with very high PV
  • Transmission thrust washers
  • Seal rings and piston rings
  • Parts for packaging and semiconductor machinery

Alternatives: Bearing-grade PEEK (lower cost, less water absorption); PI (Vespel) above 260 °C.

Frequently asked questions

Which standards cover PAI (Torlon® 4301)?

Rod, tube and sheet: Manufacturer's specification (Solvay Torlon; MCAM Duratron T4301). Machined part to drawing: ISO 2768 tolerance or as per drawing.

Up to what temperature can PAI (Torlon® 4301) be used?

Continuous service up to 260 °C, short peaks up to 270 °C; minimum -20 °C (unloaded; under load, limited by HDT and creep).

Which materials can replace PAI (Torlon® 4301)?

Bearing-grade PEEK (lower cost, less water absorption); PI (Vespel) above 260 °C.

Torlon or PEEK?

Torlon (PAI) has higher strength, stiffness and PV; PEEK absorbs less water, has better chemical resistance and costs less. For a critical bearing under high load, PAI 4301 usually wins.

Where to buy PAI (Torlon® 4301) in Brazil?

Dustre supplies PAI (Torlon® 4301) as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

Need PAI (Torlon® 4301)?Rods, sheets, tubes and parts machined to drawing, with lot certificate of conformity.

Forms and stock of PAI (Torlon® 4301)

Dustre supplies PAI (Torlon® 4301) as bar, plate and pipe and tube, cut to size, with forged and machined parts to drawing (shafts, discs, rings and blocks) and a 3.1 certificate.

Not in stock at the moment: supplied to order, with lead time in the quotation.

See the full ready-to-ship stock · Request a quote for PAI (Torlon® 4301)

Where to buy PAI (Torlon® 4301) in Brazil?

Dustre supplies PAI (Torlon® 4301) as bar, plate, tube, block and forged or machined parts, subject to availability, with a quality certificate. Head office in Osasco/SP, branches in Joinville/SC and Baixo Guandu/ES, delivery across Brazil and export worldwide (export documents and 3.1 certificate; Incoterm agreed in the quote). For a quote, message Helena, our virtual assistant on WhatsApp +55 11 98649-0075, or write to vendas@dustre.com.br.

See also

HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp

We use your data only to answer this quote. Privacy. · WhatsApp +55 11 98649-0075 · Mon–Thu 07:00–17:00 · Fri 07:00–16:00 (Brasília time)