ER80S-B2 – wire and rod for 1¼Cr-½Mo steel (F11)

1¼Cr-½Mo filler metal for ASTM A182 F11 and equivalent pipes, forgings and flanges, in boilers, steam lines and refineries.

Technical review Oct 2026 · composition per AWS A5.28/A5.28M; values marked * to be confirmed in the current edition of the standard

ClassificationER80S-B2
StandardAWS A5.28/A5.28M / ASME SFA-5.28
UNSK20900
GroupCr-Mo steel

Product forms and equivalents

ProcessClassification
TIG rod (GTAW) ER80S-B2
Solid MIG/MAG wire (GMAW) ER80S-B2
Covered electrode (SMAW) E8018-B2 – AWS A5.5
Flux-cored wire (FCAW) E81T1-B2 – AWS A5.29
Submerged arc wire (SAW) EB2 + flux – AWS A5.23
Designations and equivalents
DesignationValue
AWS ER80S-B2
Specification AWS A5.28/A5.28M / ASME SFA-5.28
UNS K20900
Others EN ISO 21952-A: W/G CrMo1Si*; AWS A5.28M: ER55S-B2

Chemical composition (%)

AWS A5.28 (% by mass, filler metal)
Elementwt. %
C 0.07 – 0.12
Mn 0.40 – 0.70
Si 0.40 – 0.70
Cr 1.20 – 1.50
Mo 0.40 – 0.65
Ni ≤ 0.20
P ≤ 0.025
S ≤ 0.025
Cu ≤ 0.35

Properties of the deposited metal

PropertyValue
Tensile strength of deposited metal ≥ 550 MPa (AWS minimum, after PWHT)
Yield strength ≥ 470 MPa (AWS minimum, after PWHT)*
Elongation ≥ 19 % (AWS minimum, after PWHT)*

Materials welded with ER80S-B2

Dissimilar joints: Also used to join F11 to carbon steel or C-½Mo (F1), adopting the preheat of the more highly alloyed material.

Why the composition differs from the base metal

Chromium and molybdenum follow F11, but carbon is kept low and silicon and manganese are dosed to deoxidize the pool. The result, after PWHT, is equivalent creep resistance with a lower risk of cold cracking.

Welding precautions

  • Preheat and interpass of about 150 to 300 °C.
  • PWHT typically between 650 and 730 °C, according to the design code.
  • TIG with pure argon; MIG/MAG with argon and 2–5 % O2 or up to 20 % CO2*. Clean, dry wire and bevel to limit hydrogen.

Frequently asked questions

What is ER80S-B2 used for?

1¼Cr-½Mo filler metal for ASTM A182 F11 and equivalent pipes, forgings and flanges, in boilers, steam lines and refineries.

Why is the composition of ER80S-B2 different from the material it welds?

Chromium and molybdenum follow F11, but carbon is kept low and silicon and manganese are dosed to deoxidize the pool. The result, after PWHT, is equivalent creep resistance with a lower risk of cold cracking.

Which covered electrode corresponds to ER80S-B2?

E8018-B2 – AWS A5.5.

What precautions apply when welding with ER80S-B2?

Preheat and interpass of about 150 to 300 °C. PWHT typically between 650 and 730 °C, according to the design code. TIG with pure argon; MIG/MAG with argon and 2–5 % O2 or up to 20 % CO2*. Clean, dry wire and bevel to limit hydrogen.

Need ER80S-B2?Send the base material, the process and the wire or rod diameter.
HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp

We use your data only to answer this quote. Privacy. · WhatsApp +55 11 98649-0075 · Mon–Thu 07:00–17:00 · Fri 07:00–16:00 (Brasília time)