Dustre
EN
Customer area

ER320LR – wire and rod for Alloy 20

Niobium-stabilized 20Cr-34Ni-2.5Mo-3.5Cu filler metal, with reduced residuals, for welding Alloy 20 in sulfuric acid plants.

Technical review Oct 2026 · composition per AWS A5.9/A5.9M; values marked * to be confirmed in the current edition of the standard

ClassificationER320LR
StandardAWS A5.9/A5.9M / ASME SFA-5.9
UNSN08022
GroupAustenitic stainless

Product forms and equivalents

ProcessClassification
TIG rod (GTAW) ER320LR
Solid MIG/MAG wire (GMAW) ER320LR
Covered electrode (SMAW) E320LR-15/-16 – AWS A5.4
Submerged arc wire (SAW) ER320LR + flux
Designations and equivalents
DesignationValue
AWS ER320LR
Specification AWS A5.9/A5.9M / ASME SFA-5.9
UNS N08022
Trade designation Alloy 20 / 20Cb-3 (designação de material)

Chemical composition (%)

AWS A5.9 (% by mass, filler metal)
Elementwt. %
C ≤ 0.025
Cr 19.0 – 21.0
Ni 32.0 – 36.0
Mo 2.0 – 3.0
Cu 3.0 – 4.0
Nb 8 × C min. – 0.40
Mn 1.5 – 2.0
Si ≤ 0.15
P ≤ 0.015
S ≤ 0.02

Properties of the deposited metal

PropertyValue
Tensile strength of deposited metal ≥ 520 MPa (AWS A5.4 minimum for E320LR, reference)
Elongation ≥ 30 % (AWS A5.4 minimum for E320LR, reference)

Materials welded with ER320LR

Why the composition differs from the base metal

The “LR” (low residuals) version has much lower carbon, silicon, phosphorus, sulfur and niobium than wrought Alloy 20. The bead is fully austenitic and high in nickel, and those elements form low-melting films that would crack the weld.

Welding precautions

  • No preheating; interpass up to 100 °C.
  • Low heat input, stringer beads and filled craters to avoid hot cracking.
  • Shielding and purging with pure argon.

Frequently asked questions

What is ER320LR used for?

Niobium-stabilized 20Cr-34Ni-2.5Mo-3.5Cu filler metal, with reduced residuals, for welding Alloy 20 in sulfuric acid plants.

Why is the composition of ER320LR different from the material it welds?

The “LR” (low residuals) version has much lower carbon, silicon, phosphorus, sulfur and niobium than wrought Alloy 20. The bead is fully austenitic and high in nickel, and those elements form low-melting films that would crack the weld.

Which covered electrode corresponds to ER320LR?

E320LR-15/-16 – AWS A5.4.

What precautions apply when welding with ER320LR?

No preheating; interpass up to 100 °C. Low heat input, stringer beads and filled craters to avoid hot cracking. Shielding and purging with pure argon.

Need ER320LR?Send the base material, the process and the wire or rod diameter.
HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp

We use your data only to answer this quote. Privacy. · WhatsApp +55 11 98649-0075 · Mon–Thu 07:00–17:00 · Fri 07:00–16:00 (Brasília time)