ER80S-B6 – wire and rod for 5Cr-½Mo steel (F5)

5Cr-½Mo filler metal for ASTM A182 F5 forgings and tubes, common in refinery furnaces and lines with sulfurous crude and hydrogen.

Technical review Oct 2026 · composition per AWS A5.28/A5.28M; values marked * to be confirmed in the current edition of the standard

ClassificationER80S-B6
StandardAWS A5.28/A5.28M / ASME SFA-5.28
UNSS50280
GroupCr-Mo steel

Product forms and equivalents

ProcessClassification
TIG rod (GTAW) ER80S-B6
Solid MIG/MAG wire (GMAW) ER80S-B6
Covered electrode (SMAW) E8015-B6 / E8016-B6 / E8018-B6 – AWS A5.5
Submerged arc wire (SAW) EB6 + flux – AWS A5.23
Designations and equivalents
DesignationValue
AWS ER80S-B6
Specification AWS A5.28/A5.28M / ASME SFA-5.28
UNS S50280
Others EN ISO 21952-A: W/G CrMo5Si*; AWS A5.28M: ER55S-B6

Chemical composition (%)

AWS A5.28 (% by mass, filler metal)
Elementwt. %
C ≤ 0.10
Mn 0.40 – 0.70
Si ≤ 0.50
Cr 4.50 – 6.00
Mo 0.45 – 0.65
Ni ≤ 0.6
P ≤ 0.025
S ≤ 0.025
Cu ≤ 0.35

Properties of the deposited metal

PropertyValue
Tensile strength of deposited metal ≥ 550 MPa (AWS minimum, after PWHT)
Yield strength ≥ 470 MPa (AWS minimum, after PWHT)*
Elongation ≥ 17 % (AWS minimum, after PWHT)*

Materials welded with ER80S-B6

Why the composition differs from the base metal

The maximum carbon of 0.10 % is lower than allowed in F5, because a bead with 5 % Cr would harden to a very high hardness. With less carbon, the martensite formed is tougher and responds better to tempering.

Welding precautions

  • Preheat and interpass of about 200 to 300 °C.
  • PWHT mandatory in most codes, typically between 705 and 760 °C.
  • Cool in a controlled way before PWHT; do not let the joint cool to room temperature without post-heating on thick parts.
  • TIG with pure argon; MIG/MAG with argon and 2–5 % O2 or up to 20 % CO2*. Clean, dry wire and bevel to limit hydrogen.

Frequently asked questions

What is ER80S-B6 used for?

5Cr-½Mo filler metal for ASTM A182 F5 forgings and tubes, common in refinery furnaces and lines with sulfurous crude and hydrogen.

Why is the composition of ER80S-B6 different from the material it welds?

The maximum carbon of 0.10 % is lower than allowed in F5, because a bead with 5 % Cr would harden to a very high hardness. With less carbon, the martensite formed is tougher and responds better to tempering.

Which covered electrode corresponds to ER80S-B6?

E8015-B6 / E8016-B6 / E8018-B6 – AWS A5.5.

What precautions apply when welding with ER80S-B6?

Preheat and interpass of about 200 to 300 °C. PWHT mandatory in most codes, typically between 705 and 760 °C. Cool in a controlled way before PWHT; do not let the joint cool to room temperature without post-heating on thick parts. TIG with pure argon; MIG/MAG with argon and 2–5 % O2 or up to 20 % CO2*. Clean, dry wire and bevel to limit hydrogen.

Need ER80S-B6?Send the base material, the process and the wire or rod diameter.
HelenaVirtual assistant · WhatsApp

Request a quote

Subject: . Fill in and send: your request goes to our technical team and we reply by email.

More details (optional): tax ID, delivery, deadline and requirements
Requirements

Drawing, list or specification. Up to 5 files and 15 MB in total.

Send via WhatsApp

We use your data only to answer this quote. Privacy. · WhatsApp +55 11 98649-0075 · Mon–Thu 07:00–17:00 · Fri 07:00–16:00 (Brasília time)